MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Mitsubishi Chemical Advanced Materials Ketron™ LSG CA30 PEEK, Extruded 30% Carbon Fiber Reinforced Polyetherether Ketone
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Carbon Fiber Filled

Material Notes: Life Science Grade stock shapes, made from 30% carbon fiber-reinforced PEEK resin. Pre-assessed for biocompatibility on both resin and shape for up to 24 hours contact with body tissue according to USP VI and ISO 10993. Exhibits excellent mechanical strength, stiffness, resistance to chemicals and repeated sterilization via all current methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.41 g/cc1.41 g/ccASTM D792
Water Absorption at Saturation 0.300 %0.300 %ASTM D570 (17)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 102102ASTM D785
Hardness, Shore D 90.090.0ISO 868
Tensile Strength 144 MPa20900 psiISO 527-1/-2 (7)
Flexural Strength 220 MPa31900 psiISO 178 (12)
Compressive Yield Strength  69.0 MPa
@Strain 1.00 %
10000 psi
@Strain 1.00 %
ISO 604 (10)
 125 MPa
@Strain 2.00 %
18100 psi
@Strain 2.00 %
ISO 604 (10)
 170 MPa
@Strain 5.00 %
24700 psi
@Strain 5.00 %
ISO 604 (10)
Shear Strength 103 MPa14900 psiASTM D732
Charpy Impact, Notched 0.500 J/cm²2.38 ft-lb/in²ISO 179-1/1eA
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1e+05 - 1.00e+7 ohm1e+05 - 1.00e+7 ohmANSI/ESD STM 11.11
Dielectric Strength 1.26 kV/mm32.0 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 µm/m-°C10.0 µin/in-°FASTM E-831 (TMA)
 25.0 µm/m-°C
@Temperature 23.0 - 100 °C
13.9 µin/in-°F
@Temperature 73.4 - 212 °F
 25.0 µm/m-°C
@Temperature 23.0 - 150 °C
13.9 µin/in-°F
@Temperature 73.4 - 302 °F
 55.0 µm/m-°C
@Temperature >=150 °C
30.6 µin/in-°F
@Temperature >=302 °F
Thermal Conductivity 0.920 W/m-K6.38 BTU-in/hr-ft²-°F
 0.922 W/m-K6.40 BTU-in/hr-ft²-°F
Melting Point 340 °C644 °FASTM D3418
Maximum Service Temperature, Air 250 °C482 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 270 °C518 °FASTM D648
Minimum Service Temperature, Air -20.0 °C-4.00 °F
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) LimitedLimited
Acids, Weak AcceptableAcceptable
Alcohols AcceptableAcceptable
Alkalies, Strong (pH 11-14) AcceptableAcceptable
Alkalies, Weak AcceptableAcceptable
Chlorinated Solvents AcceptableAcceptable
Continuous Sunlight AcceptableAcceptable
Hot Water / Steam AcceptableAcceptable
Hydrocarbons - Aliphatic AcceptableAcceptable
Hydrocarbons - Aromatic AcceptableAcceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters AcceptableAcceptable
 
Descriptive Properties
ESd categoryDissipative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Chemical Advanced Materials Ketron™ CA30 PEEK, Extruded 30% Carbon Fiber Reinforced Polyetherether Ketone
Overview of materials for Polyetheretherketone, Unreinforced
Mitsubishi Chemical Advanced Materials Ketron™ GF30 PEEK, Extruded 30% Glass-Reinforced Polyetherether Ketone
Mitsubishi Chemical Advanced Materials Ketron™ 1000 PEEK, Extruded Unfilled Polyetherether Ketone
Mitsubishi Chemical Advanced Materials Ketron™ CM CA30 PEEK Polyetheretherketone, 30% carbon fiber reinforced, compression molded

P1SM18J / 85176

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.