MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Park Aerospace Nelcote® E-765 Epoxy Prepreg, 6K 4HS IM7 Reinforced
Categories: Polymer; Thermoset; Epoxy

Material Notes: Nelcote® E-765 is a tough 250°F cure prepreg system designed to replace 350°F cure systems in aircraft structural applications. FAA-approved Design Allowable Databases are available upon request.

Key Features and Benefits:

  • Designed to replace first generation 350°F (176°C) cure systems.
  • Wide cure temperature process window of 250°F to 350°F
  • Exhibits very low void content, i.e., <2% after vacuum cure.
  • Superior fiber property translation.
  • 180°F Wet service temperature after ~250°F cure
  • Good tack and drape characteristics for 3 weeks at room temperature

Applications/Qualifications:

  • Primary Aircraft Structures
    • Fuselage
    • Wing
    • Control Surfaces
  • Secondary Aircraft Structures
    • Aircraft Frames
    • Doors
    • Shelves
    • Bulkheads

Information provided by Park Electrochemical Corp.

Key Words: EP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 903 MPa
@Temperature 21.1 °C
131000 psi
@Temperature 70.0 °F
0° Direction, Dry; Autoclave Cured; ASTM D3039-95
Tensile Modulus 75.8 GPa
@Temperature 21.1 °C
11000 ksi
@Temperature 70.0 °F
0° Direction, Dry; Autoclave Cured; ASTM D3039-95
Compressive Strength  531 MPa
@Temperature 82.2 °C
77000 psi
@Temperature 180 °F
Wet; Autoclave Cured; SACMA 1-94
 607 MPa
@Temperature 82.2 °C
88000 psi
@Temperature 180 °F
Dry; Autoclave Cured; SACMA 1-94
 758 MPa
@Temperature 21.1 °C
110000 psi
@Temperature 70.0 °F
Dry; Autoclave Cured; SACMA 1-94
Compressive Modulus  62.1 GPa
@Temperature 82.2 °C
9000 ksi
@Temperature 180 °F
Dry; Autoclave Cured; SACMA 1-94
 65.5 GPa
@Temperature 21.1 °C
9500 ksi
@Temperature 70.0 °F
Dry; Autoclave Cured; SACMA 1-94
 76.5 GPa
@Temperature 82.2 °C
11100 ksi
@Temperature 180 °F
Wet; Autoclave Cured; SACMA 1-94
Shear Strength  47.6 MPa
@Temperature 82.2 °C
6900 psi
@Temperature 180 °F
Beam, V-Notched; Wet; Autoclave Cured; ASTM D5379-93
 50.3 MPa
@Temperature 82.2 °C
7300 psi
@Temperature 180 °F
Short-Beam, Wet; Autoclave Cured; ASTM D2344
 52.4 MPa
@Temperature 82.2 °C
7600 psi
@Temperature 180 °F
Beam, V-Notched; Dry; Autoclave Cured; ASTM D5379-93
 62.1 MPa
@Temperature 21.1 °C
9000 psi
@Temperature 70.0 °F
Beam, V-Notched; Dry; Autoclave Cured; ASTM D5379-93
 64.1 MPa
@Temperature 82.2 °C
9300 psi
@Temperature 180 °F
Short-Beam, Dry; Autoclave Cured; ASTM D2344
 71.0 MPa
@Temperature 21.1 °C
10300 psi
@Temperature 70.0 °F
Short-Beam, Dry; Autoclave Cured; ASTM D2344
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month
@Temperature -17.8 °C
6.00 Month
@Temperature 0.000 °F
 
Descriptive Properties
Fabric Area Weight (g/m²)203

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hexcel® HexPly® 954-2A Curing Cyanate Resin, IM7 Fiber
Hexcel® HexPly® 8552 Epoxy Matrix, IM7 Fiber
Hexcel® HexPly® 8551-7 Epoxy Matrix, IM7 Fiber
Hexcel® HexTow® IM7 12K Intermediate Modulus Carbon Fiber (12,000 Filaments)
Solvay CYCOM® 381 Epoxy Prepreg with IM7 Uni-graphite and 148FAW Epoxy

PPARK034 / 89306

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.