MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, Hardness 65A, with 3 phr Di-Cup 40C
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: Millathane® 76 is a very suitable choice for use in products such as bushings, small copier rolls; automotive applications — bumpers, o-rings, hydraulic seals, belts, gaskets, solid tires — and many other high performance polyurethane applications. Millathane 76 can be vulcanized by sulfur or peroxide cured systems.

All information provided by TSE Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 65
 65heat aged 70 hours at 100ºC
Tensile Strength 4200 psi
 4288 psiheat aged 70 hours at 100ºC
Elongation at Break 328 %heat aged 70 hours at 100ºC
 362 %
100% Modulus 0.402 ksi
@Strain 100 %
200% Modulus 1.37 ksi
@Strain 200 %
300% Modulus 3.188 ksi
@Strain 300 %
Tear Strength 38.5 kN/m
Compression Set 16.8 %
@Temperature 70.0 °C,
Time 79200 sec
heat aged 70 hours at 100ºC
 
Processing PropertiesOriginal ValueComments
Cure Time 15.0 min
@Temperature 155 °C
 
Descriptive Properties
Formulation as Tested0.5Stearic Acid
 100Millathane 76
 20N-220
 3Di-Cup 40C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
TSE Industries Millathane® CM Millable Polyether Urethane Rubber, Hardness 65A
TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 3.0 PHR Di-Cup 40C Peroxide, Hardness 65A
Overview of materials for Nylon 66/6, 30% Glass Fiber Reinforced
Mearthane Durethane™ C 65A Polyurethane
Lubrizol Estane® 2355-75A Thermoplastic Polyurethane Elastomer

PMILL453 / 87497

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.