MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

European Chestnut Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Stains in contact with iron in damp conditions. Ring-Porous Hardwood. Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Medium
Dimensional changes when dried lumber is subjected to variations in humidity during service: Large
Resistance to fungal decay (Heartwood in ground contact): Durable (15 to 25 years)
Resistance to penetration by preservatives: Permeable
Common Applications: Interior and exterior joinery. Fencing

Key Words: Castanea sativa; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.420 - 0.490 g/cc0.0152 - 0.0177 lb/in³Earlywood
 0.560 - 0.650 g/cc0.0202 - 0.0235 lb/in³Latewood
Cell Length 1.20 mm0.0472 inMature Wood
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 3100 N697 lb (f)Side
Tensile Strength, Ultimate 132 MPa19100 psi
Modulus of Rupture 0.0750 GPa10.9 ksiStatic Bending
Flexural Modulus 8.82 GPa1280 ksiStatic Bending
Compressive Strength 49.0 MPa7110 psi
Machinability 100 %100 %Good Relative to Other Wood
Shear Strength 7.80 MPa1130 psiOrientation Unknown
Toughness 22.4 J16.5 ft-lb2 cm x 2 cm sample
Cleavage 2.60 kN/m14.8 lb/in
 
Thermal PropertiesMetricEnglishComments
Shrinkage 0.60 %0.60 %Axial; Green to Zero Moisture
 4.3 %4.3 %Radial; Green to Zero Moisture
 6.4 %6.4 %Tangential; Green to Zero Moisture
 9.4 - 14.2 %9.4 - 14.2 %Volumetric; Green to Zero Moisture
 
Descriptive Properties
ColorYellowish-brownUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
European Walnut Wood
American White Oak Wood
American Hickory Wood
European Ash Wood
European White Oak Wood

PTSE060 / 71315

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.