MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Overview of materials for Nylon 612, Impact Modified
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612); Nylon 612, Impact Modified

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 612, Impact Modified". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.820 - 1.33 g/cc0.0296 - 0.0480 lb/in³Average value: 1.06 g/cc Grade Count:27
Water Absorption 0.900 - 2.70 %0.900 - 2.70 %Average value: 1.38 % Grade Count:13
Moisture Absorption at Equilibrium 0.650 - 3.50 %0.650 - 3.50 %Average value: 1.17 % Grade Count:9
Water Absorption at Saturation 2.10 - 2.80 %2.10 - 2.80 %Average value: 2.38 % Grade Count:8
Viscosity  150000 - 150000 cP
@Temperature 280 - 280 °C
150000 - 150000 cP
@Temperature 536 - 536 °F
Average value: 150000 cP Grade Count:1
 150000 - 150000 cP
@Shear Rate 1000 - 1000 1/s
150000 - 150000 cP
@Shear Rate 1000 - 1000 1/s
Average value: 150000 cP Grade Count:1
Viscosity Number 171 - 180 cm³/g1.71 - 1.80 dl/gAverage value: 175 cm³/g Grade Count:3
Linear Mold Shrinkage 0.00200 - 0.0270 cm/cm0.00200 - 0.0270 in/inAverage value: 0.0137 cm/cm Grade Count:8
Linear Mold Shrinkage, Transverse 0.00800 - 0.0130 cm/cm0.00800 - 0.0130 in/inAverage value: 0.0102 cm/cm Grade Count:6
Melt Flow 4.20 - 60.0 g/10 min4.20 - 60.0 g/10 minAverage value: 22.3 g/10 min Grade Count:7
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 65.0 - 75.065.0 - 75.0Average value: 69.7 Grade Count:6
Ball Indentation Hardness 25.0 - 100 MPa3630 - 14500 psiAverage value: 47.6 MPa Grade Count:7
Tensile Strength, Ultimate 22.5 - 151 MPa3260 - 21900 psiAverage value: 54.5 MPa Grade Count:17
Tensile Strength, Yield 9.00 - 90.0 MPa1310 - 13100 psiAverage value: 36.2 MPa Grade Count:14
Elongation at Break 4.50 - 370 %4.50 - 370 %Average value: 117 % Grade Count:27
Elongation at Yield 5.00 - 32.0 %5.00 - 32.0 %Average value: 19.6 % Grade Count:12
Modulus of Elasticity 0.400 - 9.10 GPa58.0 - 1320 ksiAverage value: 1.75 GPa Grade Count:23
Flexural Yield Strength 16.0 - 190 MPa2320 - 27600 psiAverage value: 57.9 MPa Grade Count:10
Flexural Modulus 0.455 - 6.75 GPa66.0 - 979 ksiAverage value: 1.67 GPa Grade Count:13
Flexural Strain at Break 5.00 - 10.0 %5.00 - 10.0 %Average value: 7.94 % Grade Count:7
Poissons Ratio 0.450 - 0.4700.450 - 0.470Average value: 0.457 Grade Count:4
Izod Impact, Notched 0.290 - 0.850 J/cm0.543 - 1.59 ft-lb/inAverage value: 0.647 J/cm Grade Count:3
Izod Impact, Notched (ISO) 10.1 - 92.0 kJ/m²4.80 - 43.8 ft-lb/in²Average value: 48.8 kJ/m² Grade Count:3
 13.0 - 13.0 kJ/m²
@Temperature -40.0 - -30.0 °C
6.19 - 6.19 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 13.0 kJ/m² Grade Count:2
Charpy Impact Unnotched 8.60 - 2100 J/cm²40.9 - 9990 ft-lb/in²Average value: 9.40 J/cm² Grade Count:20
 9.70 - 2099.79 J/cm²
@Temperature -30.0 - 0.000 °C
46.2 - 9993.41 ft-lb/in²
@Temperature -22.0 - 32.0 °F
Average value: 10.3 J/cm² Grade Count:20
Charpy Impact, Notched 1.60 - 2100 J/cm²7.60 - 9990 ft-lb/in²Average value: 5.96 J/cm² Grade Count:23
 0.600 - 7.98 J/cm²
@Temperature -40.0 - 0.000 °C
2.86 - 38.0 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 1.95 J/cm² Grade Count:23
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 6.00e+7 - 1.00e+13 ohm-cm6.00e+7 - 1.00e+13 ohm-cmAverage value: 1.03e+12 ohm-cm Grade Count:16
Surface Resistance 1.00e+10 - 1.40e+14 ohm1.00e+10 - 1.40e+14 ohmAverage value: 2.63e+13 ohm Grade Count:11
Dielectric Constant 2.70 - 9.202.70 - 9.20Average value: 4.67 Grade Count:5
Dielectric Strength 26.0 - 39.0 kV/mm660 - 991 kV/inAverage value: 35.7 kV/mm Grade Count:14
Dissipation Factor 0.000400 - 0.3540.000400 - 0.354Average value: 0.105 Grade Count:5
Comparative Tracking Index 575 - 600 V575 - 600 VAverage value: 597 V Grade Count:9
 
Thermal PropertiesMetricEnglishComments
CTE, linear 101 - 250 µm/m-°C56.0 - 139 µin/in-°FAverage value: 166 µm/m-°C Grade Count:8
CTE, linear, Transverse to Flow 101 - 198 µm/m-°C56.0 - 110 µin/in-°FAverage value: 131 µm/m-°C Grade Count:7
Melting Point 135 - 218 °C275 - 424 °FAverage value: 204 °C Grade Count:18
Maximum Service Temperature, Air 100 - 150 °C212 - 302 °FAverage value: 140 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 60.0 - 213 °C140 - 415 °FAverage value: 122 °C Grade Count:15
Deflection Temperature at 1.8 MPa (264 psi) 40.0 - 196 °C104 - 385 °FAverage value: 77.9 °C Grade Count:16
Vicat Softening Point 130 - 209 °C266 - 408 °FAverage value: 185 °C Grade Count:5
Glass Transition Temp, Tg -4.00 - 50.0 °C24.8 - 122 °FAverage value: 26.5 °C Grade Count:3
Flammability, UL94 HBHBGrade Count:9
Flame Spread 80.0 mm/min3.15 in/minAverage value: 80.0 mm/min Grade Count:5
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 - 280 °C428 - 536 °FAverage value: 248 °C Grade Count:16
Mold Temperature 35.0 - 90.0 °C95.0 - 194 °FAverage value: 74.7 °C Grade Count:12
Injection Velocity 200 mm/sec7.87 in/secAverage value: 200 mm/sec Grade Count:10
Drying Temperature 75.0 - 80.0 °C167 - 176 °FAverage value: 77.9 °C Grade Count:5
Moisture Content 0.0200 - 0.0600 %0.0200 - 0.0600 %Average value: 0.0457 % Grade Count:7

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 63, 35% Glass-Filled
Overview of materials for Nylon 11, Unreinforced
Overview of materials for Nylon 66, Impact Grade
Overview of materials for Nylon 610
Overview of materials for Nylon 6, 10% Glass Fiber Filled

O2601 / 78046

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.