MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Schmolz + Bickenbach Thermodur® 2367 Superclean Hot Work Die Steel
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: Description: Thermodur® 2367 Superclean is an electro slag remelted (ESR) hot work die steel developed for applications where high temperature properties (tensile strength & thermal conductivity) are required to resist thermal fatigue and tempering

Characteristics: Excellent resistance to heat checking; Excellent resistance to wear (erosion & abrasion); Excellent high-temperature strength; Good tempering resistance; and Good toughness

Applications: High pressure die casting dies, Hot forging dies, Hot extrusion tooling, Forming dies, Plastic molds and Mandrels

Stress Relieving (Heat Treatment): 1200°F for 2 hours; Cooling: Cool slowly to 900°F in air; Hardness: <230 HB

Hardening (Heat Treatment): 1875°F- 1920°F Hold at temperature for 30 minutes; Cooling: Vacuum quench at 50°F/ min, to 1000°F then cool to below 150°F; Hardness: <55 HRC Quenched

Information provided by Schmolz + Bickenbach

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.281 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 36
@Treatment Temp. 700.0 °C,
Time 7200 sec
 45
@Treatment Temp. 650.0 °C,
Time 7200 sec
 52
@Treatment Temp. 400 °C,
Time 7200 sec
 52
@Treatment Temp. 600.0 °C,
Time 7200 sec
 55
@Treatment Temp. 500 °C,
Time 7200 sec
 55
@Treatment Temp. 550.0 °C,
Time 7200 sec
Tensile Strength 203 ksi44 HRC
 234 ksi48 HRC
 267 ksi52 HRC
Tensile Strength, Yield 171 ksi
@Strain 0.2 %
44 HRC
 193 ksi
@Strain 0.2 %
48 HRC
 225 ksi
@Strain 0.2 %
52 HRC
Elongation at Yield 12 %52 HRC
 12 %44 HRC
 13 %48 HRC
Reduction of Area 35 %52 HRC
 38 %48 HRC
 40 %44 HRC
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.60 µin/in-°F
@Temperature 21.1 - 93.3 °C
 6.90 µin/in-°F
@Temperature 21.1 - 204 °C
 7.00 µin/in-°F
@Temperature 21.1 - 399 °C
Thermal Conductivity 206 BTU-in/hr-ft²-°F
@Temperature 21.1 °C
 235 BTU-in/hr-ft²-°F
@Temperature 343 °C
 245 BTU-in/hr-ft²-°F
@Temperature 704 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 1345 - 1435 °FSoft; Cooling: Furnace 20°F/hour to 1200°F/ Then air cool; < 235 HB
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.37 %
Chromium, Cr 5.0 %
Iron, Fe >= 90.627 %
Molybdenum, Mo 3.0 %
Silicon, Si 0.40 %
Sulfur, S <= 0.0030 %
Vanadium, V 0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Latrobe LSS™ 2367 Hot Work Tool Steel
Bohler-Uddeholm BÖHLER W403 VMR® Hot Work Tool Steel
Bohler-Uddeholm BÖHLER W303 ISODISC® Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM DIEVAR® Hot Work Tool Steel
Overview of materials for Air-Hardening Steel

NSCHMO016 / 125889

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.