MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Schmolz + Bickenbach Thermodur® 2367 Superclean Hot Work Die Steel
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: Description: Thermodur® 2367 Superclean is an electro slag remelted (ESR) hot work die steel developed for applications where high temperature properties (tensile strength & thermal conductivity) are required to resist thermal fatigue and tempering

Characteristics: Excellent resistance to heat checking; Excellent resistance to wear (erosion & abrasion); Excellent high-temperature strength; Good tempering resistance; and Good toughness

Applications: High pressure die casting dies, Hot forging dies, Hot extrusion tooling, Forming dies, Plastic molds and Mandrels

Stress Relieving (Heat Treatment): 1200°F for 2 hours; Cooling: Cool slowly to 900°F in air; Hardness: <230 HB

Hardening (Heat Treatment): 1875°F- 1920°F Hold at temperature for 30 minutes; Cooling: Vacuum quench at 50°F/ min, to 1000°F then cool to below 150°F; Hardness: <55 HRC Quenched

Information provided by Schmolz + Bickenbach

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.78 g/cc0.281 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  36
@Treatment Temp. 700.0 °C,
Time 7200 sec
36
@Treatment Temp. 1292 °F,
Time 2.00 hour
 45
@Treatment Temp. 650.0 °C,
Time 7200 sec
45
@Treatment Temp. 1202 °F,
Time 2.00 hour
 52
@Treatment Temp. 400 °C,
Time 7200 sec
52
@Treatment Temp. 752 °F,
Time 2.00 hour
 52
@Treatment Temp. 600.0 °C,
Time 7200 sec
52
@Treatment Temp. 1112 °F,
Time 2.00 hour
 55
@Treatment Temp. 500 °C,
Time 7200 sec
55
@Treatment Temp. 932 °F,
Time 2.00 hour
 55
@Treatment Temp. 550.0 °C,
Time 7200 sec
55
@Treatment Temp. 1022 °F,
Time 2.00 hour
Tensile Strength 1400 MPa203000 psi44 HRC
 1610 MPa234000 psi48 HRC
 1840 MPa267000 psi52 HRC
Tensile Strength, Yield  1180 MPa
@Strain 0.2 %
171000 psi
@Strain 0.2 %
44 HRC
 1330 MPa
@Strain 0.2 %
193000 psi
@Strain 0.2 %
48 HRC
 1550 MPa
@Strain 0.2 %
225000 psi
@Strain 0.2 %
52 HRC
Elongation at Yield 12 %12 %52 HRC
 12 %12 %44 HRC
 13 %13 %48 HRC
Reduction of Area 35 %35 %52 HRC
 38 %38 %48 HRC
 40 %40 %44 HRC
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.9 µm/m-°C
@Temperature 21.1 - 93.3 °C
6.60 µin/in-°F
@Temperature 70.0 - 200 °F
 12.4 µm/m-°C
@Temperature 21.1 - 204 °C
6.90 µin/in-°F
@Temperature 70.0 - 400 °F
 12.6 µm/m-°C
@Temperature 21.1 - 399 °C
7.00 µin/in-°F
@Temperature 70.0 - 750 °F
Thermal Conductivity  29.7 W/m-K
@Temperature 21.1 °C
206 BTU-in/hr-ft²-°F
@Temperature 70.0 °F
 33.9 W/m-K
@Temperature 343 °C
235 BTU-in/hr-ft²-°F
@Temperature 650 °F
 35.3 W/m-K
@Temperature 704 °C
245 BTU-in/hr-ft²-°F
@Temperature 1300 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 729.4 - 779.4 °C1345 - 1435 °FSoft; Cooling: Furnace 20°F/hour to 1200°F/ Then air cool; < 235 HB
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 %0.37 %
Chromium, Cr 5.0 %5.0 %
Iron, Fe >= 90.627 %>= 90.627 %
Molybdenum, Mo 3.0 %3.0 %
Silicon, Si 0.40 %0.40 %
Sulfur, S <= 0.0030 %<= 0.0030 %
Vanadium, V 0.60 %0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Latrobe LSS™ 2367 Hot Work Tool Steel
Bohler-Uddeholm BÖHLER W403 VMR® Hot Work Tool Steel
Bohler-Uddeholm BÖHLER W303 ISODISC® Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM DIEVAR® Hot Work Tool Steel
Overview of materials for Air-Hardening Steel

NSCHMO016 / 125889

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.