MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Titanium Ti-6Al-2Sn-4Zr-2Mo (Ti-6-2-4-2), Sheet
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Near Alpha Titanium Alloy

Material Notes: Unspecified heat treatment. Alpha Alloy. Silicon is often added to improve creep resistance (See Ti-6242S).

Characteristics: Good elevated-temperature performance, good creep strength

Applications: High-temp jet engines. Blades, discs, spacers, seals. High performance automotive valves.

1 other heat treatment of this alloy is in MatWeb.

Key Words: Ti6Al2Sn4Zr2Mo, Ti-6242; Ti-6-2-4-2; UNS R54620
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.54 g/cc0.164 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 318318Estimated from Rockwell C.
Hardness, Knoop 346346Estimated from Rockwell C.
Hardness, Rockwell C 3434Estimated from similar materials
Hardness, Vickers 333333Estimated from Rockwell C.
Tensile Strength  710 MPa
@Temperature 540 °C
103000 psi
@Temperature 1000 °F
 830 MPa
@Temperature 371 °C
120000 psi
@Temperature 700 °F
 890 MPa
@Temperature 204 °C
129000 psi
@Temperature 399 °F
Tensile Strength, Ultimate 1010 MPa146000 psi
Tensile Strength, Yield 990 MPa144000 psi
 570 MPa
@Temperature 540 °C
82700 psi
@Temperature 1000 °F
0.2% offset
 650 MPa
@Temperature 371 °C
94300 psi
@Temperature 700 °F
0.2% offset
 760 MPa
@Temperature 204 °C
110000 psi
@Temperature 399 °F
0.2% offset
Elongation at Break 3.0 %3.0 %
 10.8 %
@Temperature 204 °C
10.8 %
@Temperature 399 °F
 11.5 %
@Temperature 371 °C
11.5 %
@Temperature 700 °F
 17.8 %
@Temperature 540 °C
17.8 %
@Temperature 1000 °F
Tensile Modulus 120 GPa17400 ksi
Compressive Yield Strength 1080 MPa157000 psi0.2 % Permanent Set
 635 MPa
@Temperature 540 °C
92100 psi
@Temperature 1000 °F
0.2% offset
 695 MPa
@Temperature 371 °C
101000 psi
@Temperature 700 °F
0.2% offset
 800 MPa
@Temperature 204 °C
116000 psi
@Temperature 399 °F
0.2% offset
Compressive Modulus 130 GPa18900 ksi
Poissons Ratio 0.320.32duplex annealed
Fracture Toughness 148 MPa-m½135 ksi-in½Plane-Strain
Shear Modulus 45.5 GPa6600 ksiCalculated
Shear Strength 690 MPa100000 psiUltimate shear strength
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000190 ohm-cm0.000190 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.70 µm/m-°C
@Temperature 20.0 - 100 °C
4.28 µin/in-°F
@Temperature 68.0 - 212 °F
 8.10 µm/m-°C
@Temperature 20.0 - 315 °C
4.50 µin/in-°F
@Temperature 68.0 - 599 °F
average
 8.10 µm/m-°C
@Temperature 20.0 - 540 °C
4.50 µin/in-°F
@Temperature 68.0 - 1000 °F
average
Specific Heat Capacity 0.460 J/g-°C0.110 BTU/lb-°F
Thermal Conductivity 7.10 W/m-K49.3 BTU-in/hr-ft²-°F
Melting Point <= 1700 °C<= 3090 °FEstimated from similar materials
Liquidus 1700 °C3090 °FEstimated from similar materials
Beta Transus 990 °C1810 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 6.0 %6.0 %
Carbon, C <= 0.050 %<= 0.050 %
Hydrogen, H <= 0.0125 %<= 0.0125 %
Iron, Fe <= 0.25 %<= 0.25 %
Molybdenum, Mo 2.0 %2.0 %
Nitrogen, N <= 0.050 %<= 0.050 %
Other, each <= 0.10 %<= 0.10 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.12 %<= 0.12 %
Titanium, Ti 88 %88 %
Zirconium, Zr 4.0 %4.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-6Al-2Sn-4Zr-2Mo (Ti-6-2-4-2), Duplex Annealed
Titanium Ti-6Al-2Sn-4Zr-2Mo-0.1Si; Duplex Annealed
Titanium Ti-6Al-4V (Grade 5), Annealed
Alcoa Deltalloy® 4032-T86 Aluminum
Titanium Ti-8Al-1Mo-1V (Ti-8-1-1) Annealed 8 hr at 790°C (1450°F)

MTA642 / 14133

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.