MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Trinseo STYRON A-TECH™ 1175 Polystyrene Resin
Categories: Polymer; Thermoplastic; Polystyrene (PS)

Material Notes: STYRON A-TECH™ 1175 advanced technology polystyrene is a high impact, environmental stress crack resistant (ESCR) resin, designed for extrusion and thermoforming applications, especially for the refrigeration industry. Based on patented technology, this resin allows for potential downgauging and scrap reduction in the thermoforming process through its combination of properties like ESCR, rigidity and thermoforming.

Main Characteristics:

  • Allows for downgauging
  • ESCR to food stuff and hydrocarbons
  • Ease of processing in extrusion and thermoforming
  • Excellent thermoforming behavior
  • Increased rigidity
Applications:
  • Large Appliance/Refrigeration liners
  • General extrusion/thermoforming applications requiring ESCR
Complies with:
  • Europe REGULATION (EC) 10/2011
  • FDA, 21 CFR.177.1640
  • Consult the regulations for complete details

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Apparent Bulk Density 0.600 g/ccGranulation 7; ISO 60
Melt Flow 2.8 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 24.0 MPaISO 527-2/5
Tensile Strength, Yield 16.0 MPaISO 527-2/5
Elongation at Break 60 %ISO 527-2/5
Tensile Modulus 1650 MPaISO 527-2/1
Flexural Strength 38.0 MPa2.0 mm/min; ISO 178
Flexural Modulus 1650 MPa2.0 mm/min; ISO 178
Izod Impact, Notched (ISO) 8.20 kJ/m²
@Temperature -20.0 °C
ISO 180/A
 11.0 kJ/m²
@Temperature 23.0 °C
ISO 180/A
Charpy Impact, Notched 11.0 kJ/m²ISO 179/1A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 80.0 °CUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 68.0 °CUnannealed; ISO 75-2/A
Vicat Softening Point 89.0 °CISO 306/B50
 100 °CISO 306/A120
Flammability, UL94 HB
@Thickness 1.50 mm
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Trinseo STYRON X-TECH™ 2175 High-Impact Polystyrene
Trinseo STYRON™ C-TECH High-Impact Polystyrene
Trinseo STYRON A-TECH™ 1210 High-Impact Polystyrene
Trinseo STYRON A-TECH™ 1200 High-Impact Polystyrene
Overview of materials for Syndiotactic Polystyrene (SPS) with Glass or Carbon Fiber

PTRINS9090 / 197563

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.