MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for High Density Polyethylene (HDPE), Blow Molding Grade
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Blow Molding Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "High Density Polyethylene (HDPE), Blow Molding Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.935 - 1.06 g/cc0.0338 - 0.0383 lb/in³Average value: 0.954 g/cc Grade Count:400
Water Absorption 0.0100 %0.0100 %Average value: 0.0100 % Grade Count:6
Moisture Absorption at Equilibrium 0.0100 - 0.0500 %0.0100 - 0.0500 %Average value: 0.0167 % Grade Count:6
Environmental Stress Crack Resistance 3.00 - 5000 hour3.00 - 5000 hourAverage value: 347 hour Grade Count:232
 10.0 - 1000 hour
@Temperature 50.0 - 80.0 °C
10.0 - 1000 hour
@Temperature 122 - 176 °F
Average value: 276 hour Grade Count:45
 13.0 - 530 hour
@Temperature 40.0 - 50.0 °C
13.0 - 530 hour
@Temperature 104 - 122 °F
Average value: 276 hour Grade Count:16
 13.0 - 530 hour
@Thickness 0.300 - 2.00 mm
13.0 - 530 hour
@Thickness 0.0118 - 0.0787 in
Average value: 276 hour Grade Count:16
Thermal Stress Crack Resistance 250 hour250 hourAverage value: 250 hour Grade Count:4
Oxidative Induction Time (OIT) 7.00 - 105 min
@Temperature 200 - 200 °C
7.00 - 105 min
@Temperature 392 - 392 °F
Average value: 41.9 min Grade Count:27
Linear Mold Shrinkage 0.0150 - 0.0500 cm/cm0.0150 - 0.0500 in/inAverage value: 0.0219 cm/cm Grade Count:4
Melt Flow 0.0100 - 57.0 g/10 min0.0100 - 57.0 g/10 minAverage value: 6.41 g/10 min Grade Count:401
Ash 0.0300 - 0.0600 %0.0300 - 0.0600 %Average value: 0.0467 % Grade Count:3
 <= 2.00 %
@Temperature 600 - 600 °C
<= 2.00 %
@Temperature 1110 - 1110 °F
Average value: 2.00 % Grade Count:6
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 50.0 - 79.050.0 - 79.0Average value: 64.3 Grade Count:167
Ball Indentation Hardness 44.0 - 63.0 MPa6380 - 9140 psiAverage value: 52.0 MPa Grade Count:7
Tensile Strength, Ultimate 11.7 - 44.0 MPa1700 - 6380 psiAverage value: 29.3 MPa Grade Count:130
Film Tensile Strength at Yield, MD 20.0 - 27.0 MPa2900 - 3920 psiAverage value: 24.7 MPa Grade Count:11
Film Tensile Strength at Yield, TD 19.0 - 30.0 MPa2760 - 4350 psiAverage value: 22.7 MPa Grade Count:12
Tensile Strength, Yield 15.2 - 43.0 MPa2200 - 6240 psiAverage value: 27.2 MPa Grade Count:333
Film Elongation at Break, MD 240 - 810 %240 - 810 %Average value: 560 % Grade Count:15
Film Elongation at Break, TD 350 - 980 %350 - 980 %Average value: 625 % Grade Count:15
Elongation at Break 7.00 - 2000 %7.00 - 2000 %Average value: 707 % Grade Count:275
Elongation at Yield 4.00 - 13.0 %4.00 - 13.0 %Average value: 9.04 % Grade Count:97
Modulus of Elasticity 0.650 - 4.30 GPa94.3 - 624 ksiAverage value: 1.28 GPa Grade Count:47
Flexural Modulus 0.120 - 2.62 GPa17.4 - 380 ksiAverage value: 1.25 GPa Grade Count:310
Secant Modulus 0.900 - 1.36 GPa131 - 197 ksiAverage value: 1.02 GPa Grade Count:6
Izod Impact, Notched 0.250 - 5340 J/cm0.468 - 10000 ft-lb/inAverage value: 3.33 J/cm Grade Count:87
Izod Impact, Unnotched 2.70 - 7.20 J/cm5.06 - 13.5 ft-lb/inAverage value: 4.96 J/cm Grade Count:9
Izod Impact, Notched (ISO) 8.00 - 24.0 kJ/m²3.81 - 11.4 ft-lb/in²Average value: 13.5 kJ/m² Grade Count:29
Charpy Impact Unnotched 0.600 - 0.650 J/cm²
@Temperature -30.0 - -30.0 °C
2.86 - 3.09 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 0.625 J/cm² Grade Count:2
Charpy Impact, Notched 0.400 J/cm² - NB1.90 ft-lb/in² - NBAverage value: 1.98 J/cm² Grade Count:20
 0.250 - 5.50 J/cm²
@Temperature -30.0 - -30.0 °C
1.19 - 26.2 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 1.43 J/cm² Grade Count:15
Tensile Impact Strength 50.0 - 4800 kJ/m²23.8 - 2280 ft-lb/in²Average value: 270 kJ/m² Grade Count:91
 65.0 - 399 kJ/m²
@Temperature -40.0 - -30.0 °C
30.9 - 190 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 151 kJ/m² Grade Count:10
Tensile Impact 53.4 - 131 J/cm100 - 245 ft-lb/inAverage value: 77.4 J/cm Grade Count:25
Tensile Creep Modulus, 1 hour 360 - 510 MPa52200 - 74000 psiAverage value: 413 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 250 - 340 MPa36300 - 49300 psiAverage value: 282 MPa Grade Count:6
Tear Strength Test 23.5 - 30.023.5 - 30.0Average value: 28.4 Grade Count:4
Elmendorf Tear Strength MD 12.0 - 25.0 g12.0 - 25.0 gAverage value: 18.0 g Grade Count:14
Elmendorf Tear Strength TD 25.0 - 260 g25.0 - 260 gAverage value: 146 g Grade Count:15
Dart Drop Test 20.0 - 350 g0.0441 - 0.772 lbAverage value: 153 g Grade Count:15
Film Tensile Strength at Break, MD 39.0 - 68.9 MPa5660 - 10000 psiAverage value: 56.6 MPa Grade Count:15
Film Tensile Strength at Break, TD 25.0 - 67.6 MPa3630 - 9800 psiAverage value: 42.4 MPa Grade Count:15
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 10000 - 1.00e+15 ohm-cm10000 - 1.00e+15 ohm-cmAverage value: 8.57e+14 ohm-cm Grade Count:7
Surface Resistance 10000 - 1.00e+14 ohm10000 - 1.00e+14 ohmAverage value: 8.57e+13 ohm Grade Count:7
Dielectric Constant 2.402.40Average value: 2.40 Grade Count:6
Dielectric Strength 150 kV/mm3810 kV/inAverage value: 150 kV/mm Grade Count:6
Dissipation Factor 0.0002000.000200Average value: 0.000200 Grade Count:6
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:6
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 - 170 µm/m-°C10.0 - 94.4 µin/in-°FAverage value: 121 µm/m-°C Grade Count:17
Melting Point 26.0 - 269 °C78.8 - 516 °FAverage value: 131 °C Grade Count:51
Crystallization Temperature 108 - 120 °C226 - 248 °FAverage value: 116 °C Grade Count:14
Deflection Temperature at 0.46 MPa (66 psi) 48.0 - 99.0 °C118 - 210 °FAverage value: 72.9 °C Grade Count:134
Deflection Temperature at 1.8 MPa (264 psi) 42.0 - 46.0 °C108 - 115 °FAverage value: 43.7 °C Grade Count:6
Vicat Softening Point 62.0 - 131 °C144 - 268 °FAverage value: 123 °C Grade Count:211
Softening Point 70.0 - 80.0 °C158 - 176 °FAverage value: 76.8 °C Grade Count:4
Heat Distortion Temperature 38.0 - 75.0 °C100 - 167 °FAverage value: 58.2 °C Grade Count:3
Brittleness Temperature -118 - 82.2 °C-180 - 180 °FAverage value: -80.7 °C Grade Count:185
Flammability, UL94 HB - V-2HB - V-2Grade Count:7
Oxygen Index 17.0 %17.0 %Average value: 17.0 % Grade Count:6
 
Optical PropertiesMetricEnglishComments
Gloss 25.0 - 90.0 %25.0 - 90.0 %Average value: 41.7 % Grade Count:3
 
Processing PropertiesMetricEnglishComments
Processing Temperature 157 - 250 °C315 - 482 °FAverage value: 198 °C Grade Count:53
Die Temperature 5.00 - 220 °C41.0 - 428 °FAverage value: 182 °C Grade Count:15
Melt Temperature 130 - 280 °C266 - 536 °FAverage value: 193 °C Grade Count:60
Head Temperature 185 - 204 °C365 - 399 °FAverage value: 194 °C Grade Count:3
Mold Temperature 5.00 - 40.0 °C41.0 - 104 °FAverage value: 19.4 °C Grade Count:8

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for High Density Polyethylene (HDPE), Injection Molded
Overview of materials for High Density Polyethylene (HDPE), Extruded
Overview of materials for Low Density Polyethylene (LDPE), Blow Molding Grade
Overview of materials for High Density Polyethylene (HDPE), Film Grade
Overview of materials for High Density Polyethylene (HDPE), Pipe Grade

O4006 / 78281

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.