MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Crucible Steel CPM® 3V® Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel

Material Notes: CPM 3V is a new tool steel made by the Crucible Particle Metallurgy process, designed to provide maximum resistance to breakage and chipping in a highly wear-resistant steel. CPM 3V offers impact toughness greater than A2, D2, Cru-Wear or CPM M4, approaching the levels of S7 and other shock resistant grades, while providing excellent wear resistance, high hardness and thermal stability for coatings. Intended to be used at HRC 58-60 CPM 3V can replace high alloy tool steels in wear applications where chronic tool breakage and chipping problems are encountered.

The CPM process produces very homogeneous, high quality steel characterized by superior dimensional stability, grindability, and toughness compared to steels produced by conventional processes.

Information provided by Crucible Specialty Metals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 241241Annealed
Hardness, Rockwell C 58 - 6058 - 60
Modulus of Elasticity 207 GPa30000 ksi
Charpy Impact 53.0 J39.1 ft-lbAustenitizing Temperature- 1120°C
 95.0 J70.1 ft-lbAustenitizing Temperature- 1065°C
 113 J83.3 ft-lbAustenitizing Temperature- 1025°C
 
Thermal PropertiesMetricEnglishComments
CTE, linear 10.6 µm/m-°C
@Temperature 20.0 - 200 °C
5.89 µin/in-°F
@Temperature 68.0 - 392 °F
Thermal Conductivity 24.2 W/m-K
@Temperature 200 °C
168 BTU-in/hr-ft²-°F
@Temperature 392 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.80 %0.80 %
Chromium, Cr 7.5 %7.5 %
Iron, Fe 88.65 %88.65 %As Remainder
Molybdenum, Mo 1.3 %1.3 %
Vanadium, V 2.75 %2.75 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Crucible Steel CPM® 9V® Tool Steel
Crucible Steel CPM® Rex M4 HC(HS) Tool Steel
AISI Type M4 Molybdenum High Speed Tool Steel (UNS T11304)
Crucible Steel REX® M4 High Speed Steel
Carpenter Four Star High Speed Steel Red-Wear® (AISI M4)

NCRUC001 / 15994

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.