MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 66, 40% Mineral Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, 40% Mineral Filled". Specific grades with primary filler content between 35% and 44% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.32 - 1.67 g/cc0.0477 - 0.0603 lb/in³Average value: 1.49 g/cc Grade Count:125
 1.27 - 1.28 g/cc
@Temperature >=256 °C
0.0459 - 0.0462 lb/in³
@Temperature >=493 °F
Average value: 1.27 g/cc Grade Count:2
Filler Content 40.0 - 43.0 %40.0 - 43.0 %Average value: 40.1 % Grade Count:22
Water Absorption 0.0700 - 5.80 %0.0700 - 5.80 %Average value: 2.32 % Grade Count:60
Moisture Absorption at Equilibrium 1.00 - 2.00 %1.00 - 2.00 %Average value: 1.53 % Grade Count:29
Water Absorption at Saturation 4.00 - 7.00 %4.00 - 7.00 %Average value: 4.73 % Grade Count:10
Maximum Moisture Content 0.0200 - 0.2000.0200 - 0.200Average value: 0.0825 Grade Count:4
Linear Mold Shrinkage 0.00200 - 0.0170 cm/cm0.00200 - 0.0170 in/inAverage value: 0.00891 cm/cm Grade Count:99
Linear Mold Shrinkage, Transverse 0.00400 - 0.0200 cm/cm0.00400 - 0.0200 in/inAverage value: 0.0104 cm/cm Grade Count:43
Melt Flow 1.00 - 10.0 g/10 min1.00 - 10.0 g/10 minAverage value: 4.17 g/10 min Grade Count:6
Ash 40.0 %40.0 %Average value: 40.0 % Grade Count:4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 86.0 - 97.086.0 - 97.0Average value: 93.8 Grade Count:10
Hardness, Rockwell R 105 - 122105 - 122Average value: 120 Grade Count:20
Ball Indentation Hardness 155 - 260 MPa22500 - 37700 psiAverage value: 220 MPa Grade Count:4
Tensile Strength, Ultimate 45.0 - 105 MPa6530 - 15200 psiAverage value: 80.5 MPa Grade Count:97
 20.0 - 65.0 MPa
@Temperature 60.0 - 150 °C
2900 - 9430 psi
@Temperature 140 - 302 °F
Average value: 45.8 MPa Grade Count:4
Tensile Strength, Yield 68.9 - 200 MPa10000 - 29000 psiAverage value: 93.0 MPa Grade Count:33
Elongation at Break 1.00 - 75.0 %1.00 - 75.0 %Average value: 6.53 % Grade Count:104
 2.50 - 25.0 %
@Temperature 60.0 - 190 °C
2.50 - 25.0 %
@Temperature 140 - 374 °F
Average value: 12.4 % Grade Count:1
Elongation at Yield 1.50 - 35.0 %1.50 - 35.0 %Average value: 5.89 % Grade Count:15
 6.00 - 10.0 %
@Temperature 90.0 - 150 °C
6.00 - 10.0 %
@Temperature 194 - 302 °F
Average value: 8.67 % Grade Count:1
Modulus of Elasticity 0.400 - 10.0 GPa58.0 - 1450 ksiAverage value: 6.38 GPa Grade Count:58
 1.60 - 7.30 GPa
@Temperature 60.0 - 150 °C
232 - 1060 ksi
@Temperature 140 - 302 °F
Average value: 3.70 GPa Grade Count:1
Flexural Yield Strength 13.8 - 310 MPa2000 - 45000 psiAverage value: 138 MPa Grade Count:83
Flexural Modulus 2.00 - 11.4 GPa290 - 1650 ksiAverage value: 6.51 GPa Grade Count:101
 1.10 - 5.20 GPa
@Temperature 60.0 - 120 °C
160 - 754 ksi
@Temperature 140 - 248 °F
Average value: 2.43 GPa Grade Count:4
Poissons Ratio 0.340 - 0.4000.340 - 0.400Average value: 0.359 Grade Count:9
Izod Impact, Notched 0.250 - 1.60 J/cm0.468 - 3.00 ft-lb/inAverage value: 0.502 J/cm Grade Count:58
 0.250 - 0.300 J/cm
@Temperature -40.0 - -20.0 °C
0.468 - 0.562 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 0.275 J/cm Grade Count:1
Izod Impact, Unnotched 0.374 - 7.47 J/cm0.700 - 14.0 ft-lb/inAverage value: 3.28 J/cm Grade Count:13
Izod Impact, Notched (ISO) 3.00 - 150 kJ/m²1.43 - 71.4 ft-lb/in²Average value: 8.67 kJ/m² Grade Count:36
 2.00 - 100 kJ/m²
@Temperature -40.0 - -30.0 °C
0.952 - 47.6 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 21.3 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) 3.50 - 95.0 kJ/m²1.67 - 45.2 ft-lb/in²Average value: 24.8 kJ/m² Grade Count:8
 4.00 - 18.0 kJ/m²
@Temperature -40.0 - -30.0 °C
1.90 - 8.57 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 7.72 kJ/m² Grade Count:3
Charpy Impact Unnotched 1.50 - 2100 J/cm²7.14 - 9990 ft-lb/in²Average value: 5.94 J/cm² Grade Count:42
 1.10 - 13.0 J/cm²
@Temperature -40.0 - -20.0 °C
5.24 - 61.9 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 4.23 J/cm² Grade Count:31
Charpy Impact, Notched 0.200 - 1.70 J/cm²0.952 - 8.09 ft-lb/in²Average value: 0.572 J/cm² Grade Count:55
 0.150 - 0.800 J/cm²
@Temperature -40.0 - -20.0 °C
0.714 - 3.81 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 0.331 J/cm² Grade Count:32
Tensile Creep Modulus, 1 hour 2100 - 8500 MPa305000 - 1.23e+6 psiAverage value: 4550 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 1300 - 2100 MPa189000 - 305000 psiAverage value: 1600 MPa Grade Count:4
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+10 - 1.00e+17 ohm-cm1.00e+10 - 1.00e+17 ohm-cmAverage value: 5.00e+15 ohm-cm Grade Count:46
Surface Resistance 1.00e+10 - 1.00e+15 ohm1.00e+10 - 1.00e+15 ohmAverage value: 1.39e+14 ohm Grade Count:25
Dielectric Constant 3.20 - 12.63.20 - 12.6Average value: 5.28 Grade Count:16
Dielectric Strength 15.0 - 85.0 kV/mm380 - 2160 kV/inAverage value: 30.8 kV/mm Grade Count:39
Dissipation Factor 0.00200 - 0.4400.00200 - 0.440Average value: 0.0823 Grade Count:14
Comparative Tracking Index 300 - 600 V300 - 600 VAverage value: 539 V Grade Count:32
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.20 - 90.0 µm/m-°C4.00 - 50.0 µin/in-°FAverage value: 45.1 µm/m-°C Grade Count:29
 63.0 - 63.0 µm/m-°C
@Temperature 35.0 - 55.0 °C
35.0 - 35.0 µin/in-°F
@Temperature 95.0 - 131 °F
Average value: 63.0 µm/m-°C Grade Count:1
 63.0 - 63.0 µm/m-°C
@Thickness 2.00 - 2.00 mm
35.0 - 35.0 µin/in-°F
@Thickness 0.0787 - 0.0787 in
Average value: 63.0 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 40.0 - 90.0 µm/m-°C22.2 - 50.0 µin/in-°FAverage value: 65.2 µm/m-°C Grade Count:13
Specific Heat Capacity 1.90 - 1.90 J/g-°C
@Temperature >=256 °C
0.454 - 0.454 BTU/lb-°F
@Temperature >=493 °F
Average value: 1.90 J/g-°C Grade Count:1
Thermal Conductivity 0.270 - 0.270 W/m-K
@Temperature >=256 °C
1.87 - 1.87 BTU-in/hr-ft²-°F
@Temperature >=493 °F
Average value: 0.270 W/m-K Grade Count:1
Melting Point 221 - 325 °C430 - 617 °FAverage value: 259 °C Grade Count:71
Maximum Service Temperature, Air 80.0 - 270 °C176 - 518 °FAverage value: 141 °C Grade Count:8
Deflection Temperature at 0.46 MPa (66 psi) 124 - 260 °C255 - 500 °FAverage value: 234 °C Grade Count:56
Deflection Temperature at 1.8 MPa (264 psi) 90.0 - 257 °C194 - 495 °FAverage value: 176 °C Grade Count:113
Vicat Softening Point 200 - 265 °C392 - 509 °FAverage value: 237 °C Grade Count:20
Flammability, UL94 HB - V-0HB - V-0Grade Count:65
Flame Spread 0.000 - 80.0 mm/min0.000 - 3.15 in/minAverage value: 71.1 mm/min Grade Count:9
Oxygen Index 23.0 - 46.5 %23.0 - 46.5 %Average value: 27.5 % Grade Count:12
Glow Wire Test 650 - 960 °C1200 - 1760 °FAverage value: 775 °C Grade Count:14
 
Processing PropertiesMetricEnglishComments
Processing Temperature 260 - 300 °C500 - 572 °FAverage value: 283 °C Grade Count:7
Nozzle Temperature 263 - 310 °C505 - 590 °FAverage value: 286 °C Grade Count:10
Melt Temperature 241 - 310 °C465 - 590 °FAverage value: 286 °C Grade Count:55
Mold Temperature 54.0 - 120 °C129 - 248 °FAverage value: 89.0 °C Grade Count:60
Drying Temperature 60.0 - 100 °C140 - 212 °FAverage value: 81.6 °C Grade Count:48
Moisture Content 0.0500 - 0.200 %0.0500 - 0.200 %Average value: 0.186 % Grade Count:27
Dew Point -17.8 °C0.000 °FAverage value: -17.8 °C Grade Count:3
Injection Pressure 30.0 - 138 MPa4350 - 20000 psiAverage value: 89.8 MPa Grade Count:19

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 10% Mineral Filled
Overview of materials for Nylon 66, 30% Mineral Filled
Overview of materials for Nylon 66, 20% Mineral Filled
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Dry)
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Conditioned)

O2534 / 78031

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.