MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay METLBOND® 1515-4 Epoxy Film Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: Metlbond 1515-4 is a 350°F (177°C) curing modified epoxy supported film adhesives. Metlbond 1515-4 can also be cured at 250°F (121°C). Its maximum continuous service temperature range is 275°F to 320°F (135°C to 160°C). Metlbond 1515-4 is commonly used for Boeing BMS 5-154 metal-to-metal and composite bonding and BMS 8-341 cosmetic surfacing.

Features & Benefits:

  • Extended shop life of 30 days at up to 90°F (32°C) allows lay up of large components
  • Designed for co-curing, secondary bonding, and co-bonding of composite materials
  • Provides excellent surfacing characteristics
  • Good resistance to pre-cure humidity
  • Available in a variety of weights and carriers
  • Bonds metal-to-metal, metal-to-core and composites
  • Co-Note 1: Metlbond 1515-4, BMS 5-154, Pre-exposed Film 30 days at 90°F (32°C) and 50% R.H.cures with most 350°F (177°C) curing prepregs
  • Storage life of 12 months at 0°F (-18°C)
Applications:
  • Metal-to-metal bonding
  • Composite bonding
  • Cosmetic surfacing
Note 1: Metlbond 1515-4, BMS 5-154, Pre-exposed Film 30 days at 90°F (32°C) and 50% R.H.

Note 2: Metlbond 1515-4, BMS 5-154, Non Pre-exposed Film

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles <= 1.0 %<= 1.0 %
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  4.22 MPa
@Temperature 71.0 °C
612 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 2, Grade 03, 14 days at 160°F (71°C), 100% R.H.
 4.85 MPa
@Temperature 71.0 °C
704 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 1, Grade 03, 14 days at 160°F (71°C), 100% R.H.
 5.17 MPa
@Temperature 71.0 °C
750 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 2, Grade 05, 14 days at 160°F (71°C), 100% R.H.
 5.48 MPa
@Temperature 71.0 °C
795 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 2, Grade 03
 5.66 MPa
@Temperature -54.0 °C
821 psi
@Temperature -65.2 °F
Honeycomb Flatwise, Note 1, Grade 03
 5.77 MPa
@Temperature 71.0 °C
837 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 1, Grade 05, 14 days at 160°F (71°C), 100% R.H.
 6.09 MPa
@Temperature -54.0 °C
883 psi
@Temperature -65.2 °F
Honeycomb Flatwise, Note 1, Grade 05
 6.11 MPa
@Temperature -54.0 °C
886 psi
@Temperature -65.2 °F
Honeycomb Flatwise, Note 2, Grade 03
 6.11 MPa
@Temperature 71.0 °C
886 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 1, Grade 03
 6.32 MPa
@Temperature 24.0 °C
916 psi
@Temperature 75.2 °F
Honeycomb Flatwise, Note 2, Grade 03
 6.45 MPa
@Temperature 24.0 °C
936 psi
@Temperature 75.2 °F
Honeycomb Flatwise, Note 1, Grade 03
 6.88 MPa
@Temperature 71.0 °C
998 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 1, Grade 05
 6.909 MPa
@Temperature 71.0 °C
1002 psi
@Temperature 160 °F
Honeycomb Flatwise, Note 2, Grade 05
 7.040 MPa
@Temperature -54.0 °C
1021 psi
@Temperature -65.2 °F
Honeycomb Flatwise, Note 2, Grade 05
 7.184 MPa
@Temperature 24.0 °C
1042 psi
@Temperature 75.2 °F
Honeycomb Flatwise, Note 1, Grade 05
 7.522 MPa
@Temperature 24.0 °C
1091 psi
@Temperature 75.2 °F
Honeycomb Flatwise, Note 2, Grade 05
Shear Strength  4.27 MPa
@Temperature 71.0 °C
620 psi
@Temperature 160 °F
Sandwich Beam, Note 2, Grade 03
 4.43 MPa
@Temperature 71.0 °C
642 psi
@Temperature 160 °F
Sandwich Beam, Note 1, Grade 03
 4.43 MPa
@Temperature 71.0 °C
643 psi
@Temperature 160 °F
Sandwich Beam, Note 1, Grade 05
 4.49 MPa
@Temperature 71.0 °C
651 psi
@Temperature 160 °F
Sandwich Beam, Note 2, Grade 05
 4.67 MPa
@Temperature 24.0 °C
678 psi
@Temperature 75.2 °F
Sandwich Beam, Note 1, Grade 03
 4.84 MPa
@Temperature 24.0 °C
702 psi
@Temperature 75.2 °F
Sandwich Beam, Note 1, Grade 05
 4.85 MPa
@Temperature 24.0 °C
704 psi
@Temperature 75.2 °F
Sandwich Beam, Note 2, Grade 05
 4.91 MPa
@Temperature 24.0 °C
712 psi
@Temperature 75.2 °F
Sandwich Beam, Note 2, Grade 03
 5.06 MPa
@Temperature -54.0 °C
734 psi
@Temperature -65.2 °F
Sandwich Beam, Note 1, Grade 03
 5.23 MPa
@Temperature -54.0 °C
759 psi
@Temperature -65.2 °F
Sandwich Beam, Note 1, Grade 05
 5.32 MPa
@Temperature -54.0 °C
771 psi
@Temperature -65.2 °F
Sandwich Beam, Note 2, Grade 03
 5.35 MPa
@Temperature -54.0 °C
776 psi
@Temperature -65.2 °F
Sandwich Beam, Note 2, Grade 05
 11.05 MPa
@Temperature 132 °C
1602 psi
@Temperature 270 °F
Double Lap, Note 1, Grade 05
 11.91 MPa
@Temperature 132 °C
1728 psi
@Temperature 270 °F
Double Lap, Note 1, Grade 03
 13.39 MPa
@Temperature 132 °C
1942 psi
@Temperature 270 °F
Double Lap, Note 2, Grade 03
 13.95 MPa
@Temperature 132 °C
2023 psi
@Temperature 270 °F
Double Lap, Note 2, Grade 05
 22.12 MPa
@Temperature 71.0 °C
3208 psi
@Temperature 160 °F
Double Lap, Note 2, Grade 05, 14 days at 160°F (71°C), 100% R.H.
 23.46 MPa
@Temperature 71.0 °C
3402 psi
@Temperature 160 °F
Double Lap, Note 1, Grade 05, 14 days at 160°F (71°C), 100% R.H.
 23.6 MPa
@Temperature 71.0 °C
3420 psi
@Temperature 160 °F
Double Lap, Note 2, Grade 03, 14 days at 160°F (71°C), 100% R.H.
 23.84 MPa
@Temperature -54.0 °C
3458 psi
@Temperature -65.2 °F
Double Lap, Note 1, Grade 05
 24.10 MPa
@Temperature -54.0 °C
3495 psi
@Temperature -65.2 °F
Double Lap, Note 2, Grade 05
 25.70 MPa
@Temperature -54.0 °C
3727 psi
@Temperature -65.2 °F
Double Lap, Note 1, Grade 03
 25.71 MPa
@Temperature 71.0 °C
3729 psi
@Temperature 160 °F
Double Lap, Note 1, Grade 03, 14 days at 160°F (71°C), 100% R.H.
 27.06 MPa
@Temperature -54.0 °C
3925 psi
@Temperature -65.2 °F
Double Lap, Note 2, Grade 03
 27.80 MPa
@Temperature 71.0 °C
4032 psi
@Temperature 160 °F
Double Lap, Note 2, Grade 03
 28.5 MPa
@Temperature 71.0 °C
4130 psi
@Temperature 160 °F
Double Lap, Note 1, Grade 05
 28.55 MPa
@Temperature 71.0 °C
4141 psi
@Temperature 160 °F
Double Lap, Note 2, Grade 05
 30.21 MPa
@Temperature 71.0 °C
4381 psi
@Temperature 160 °F
Double Lap, Note 1, Grade 08, 14 days at 160°F (71°C), 100% R.H.
 31.6 MPa
@Temperature 71.0 °C
4590 psi
@Temperature 160 °F
Double Lap, Note 2, Grade 08, 14 days at 160°F (71°C), 100% R.H.
 31.75 MPa
@Temperature 71.0 °C
4605 psi
@Temperature 160 °F
Double Lap, Note 1, Grade 03
 32.43 MPa
@Temperature 24.0 °C
4703 psi
@Temperature 75.2 °F
Double Lap, Note 1, Grade 03
 32.46 MPa
@Temperature 24.0 °C
4708 psi
@Temperature 75.2 °F
Double Lap, Note 2, Grade 05
 32.71 MPa
@Temperature 24.0 °C
4744 psi
@Temperature 75.2 °F
Double Lap, Note 1, Grade 08
 32.76 MPa
@Temperature 24.0 °C
4752 psi
@Temperature 75.2 °F
Double Lap, Note 1, Grade 05
 34.08 MPa
@Temperature 24.0 °C
4943 psi
@Temperature 75.2 °F
Double Lap, Note 2, Grade 03
 45.27 MPa
@Temperature 24.0 °C
6566 psi
@Temperature 75.2 °F
Double Lap, Note 2, Grade 08
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 160 °C320 °F
Minimum Service Temperature, Air -54.0 °C-65.2 °F
Glass Transition Temp, Tg 170 °C338 °F
 
Descriptive Properties
ColorBlue

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay METLBOND® 1146-3 Epoxy Film Adhesive
Solvay METLBOND® 1515-3 Film Adhesive
Elantas Conap FR-1210 / EA-117 Conapoxy® Resin / Conacure® Hardener
Elantas Conap FR-1200 / EA-117 Conapoxy® Resin / Conacure® Hardener
Elantas Conap FR-1080 Conapoxy® Resin / Conacure® Hardener

PCYTED052 / 180354

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.