Physical Properties | Metric | English | Comments |
---|
Density | 3.53 g/cc | 0.128 lb/in³ |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 53 | 53 |
Alkali Class, AR | 1.3 | 1.3 |
Stain Resistance Class, FR | 2.0 | 2.0 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 721 | 721 |
Modulus of Elasticity | 108 GPa | 15700 ksi |
Poissons Ratio | 0.288 | 0.288 |
Shear Modulus | 41.9 GPa | 6080 ksi |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 6.30 µm/m-°C @Temperature -30.0 - 70.0 °C | 3.50 µin/in-°F @Temperature -22.0 - 158 °F |
| 7.60 µm/m-°C @Temperature 20.0 - 300 °C | 4.22 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.660 J/g-°C | 0.158 BTU/lb-°F |
Thermal Conductivity | 0.880 W/m-K | 6.11 BTU-in/hr-ft²-°F |
Transformation Temperature, Tg | 634 °C | 1170 °F |
Softening Point | 710 °C | 1310 °F |
Annealing Point | 635 °C | 1180 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.653 @Wavelength 2325.4 nm | 1.653 @Wavelength 2325.4 nm |
| 1.66 @Wavelength 1970.1 nm | 1.66 @Wavelength 1970.1 nm |
| 1.667 @Wavelength 1529.6 nm | 1.667 @Wavelength 1529.6 nm |
| 1.673 @Wavelength 1014 nm | 1.673 @Wavelength 1014 nm |
| 1.675 @Wavelength 1060 nm | 1.675 @Wavelength 1060 nm |
| 1.679 @Wavelength 852.1 nm | 1.679 @Wavelength 852.1 nm |
| 1.684 @Wavelength 706.5 nm | 1.684 @Wavelength 706.5 nm |
| 1.686 @Wavelength 656.3 nm | 1.686 @Wavelength 656.3 nm |
| 1.687 @Wavelength 632.8 nm | 1.687 @Wavelength 632.8 nm |
| 1.687 @Wavelength 643.8 nm | 1.687 @Wavelength 643.8 nm |
| 1.69 @Wavelength 589.3 nm | 1.69 @Wavelength 589.3 nm |
| 1.69 @Wavelength 587.6 nm | 1.69 @Wavelength 587.6 nm |
| 1.693 @Wavelength 546.1 nm | 1.693 @Wavelength 546.1 nm |
| 1.699 @Wavelength 486.1 nm | 1.699 @Wavelength 486.1 nm |
| 1.70 @Wavelength 480 nm | 1.70 @Wavelength 480 nm |
| 1.706 @Wavelength 435.8 nm | 1.706 @Wavelength 435.8 nm |
| 1.712 @Wavelength 404.7 nm | 1.712 @Wavelength 404.7 nm |
Abbe Number | 54.53 | 54.53 |
| 54.76 | 54.76 |
Optical Dispersion | 0.012612 | 0.012612 |
| 0.012721 | 0.012721 |
Transmission, Visible | 32 % @Thickness 25.0 mm, Wavelength 420 nm | 32 % @Thickness 0.984 in, Wavelength 420 nm |
| 57 % @Thickness 25.0 mm, Wavelength 436 nm | 57 % @Thickness 0.984 in, Wavelength 436 nm |
| 63.4 % @Thickness 10.0 mm, Wavelength 420 nm | 63.4 % @Thickness 0.394 in, Wavelength 420 nm |
| 79.9 % @Thickness 10.0 mm, Wavelength 436 nm | 79.9 % @Thickness 0.394 in, Wavelength 436 nm |
| 81 % @Thickness 25.0 mm, Wavelength 460 nm | 81 % @Thickness 0.984 in, Wavelength 460 nm |
| 91.9 % @Thickness 10.0 mm, Wavelength 460 nm | 91.9 % @Thickness 0.394 in, Wavelength 460 nm |
| 93 % @Thickness 25.0 mm, Wavelength 500 nm | 93 % @Thickness 0.984 in, Wavelength 500 nm |
| 96.4 % @Thickness 25.0 mm, Wavelength 546 nm | 96.4 % @Thickness 0.984 in, Wavelength 546 nm |
| 97.1 % @Thickness 10.0 mm, Wavelength 500 nm | 97.1 % @Thickness 0.394 in, Wavelength 500 nm |
| 97.3 % @Thickness 25.0 mm, Wavelength 580 nm | 97.3 % @Thickness 0.984 in, Wavelength 580 nm |
| 97.8 % @Thickness 25.0 mm, Wavelength 620 nm | 97.8 % @Thickness 0.984 in, Wavelength 620 nm |
| 98.2 % @Thickness 25.0 mm, Wavelength 660 nm | 98.2 % @Thickness 0.984 in, Wavelength 660 nm |
| 98.5 % @Thickness 10.0 mm, Wavelength 546 nm | 98.5 % @Thickness 0.394 in, Wavelength 546 nm |
| 98.6 % @Thickness 25.0 mm, Wavelength 700 nm | 98.6 % @Thickness 0.984 in, Wavelength 700 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 580 nm | 98.9 % @Thickness 0.394 in, Wavelength 580 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 620 nm | 99.1 % @Thickness 0.394 in, Wavelength 620 nm |
| 99.3 % @Thickness 10.0 mm, Wavelength 660 nm | 99.3 % @Thickness 0.394 in, Wavelength 660 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 700 nm | 99.4 % @Thickness 0.394 in, Wavelength 700 nm |
IR Transmittance | 16 % @Thickness 25.0 mm, Wavelength 2500 nm | 16 % @Thickness 0.984 in, Wavelength 2500 nm |
| 48 % @Thickness 10.0 mm, Wavelength 2500 nm | 48 % @Thickness 0.394 in, Wavelength 2500 nm |
| 49 % @Thickness 25.0 mm, Wavelength 2325 nm | 49 % @Thickness 0.984 in, Wavelength 2325 nm |
| 75.2 % @Thickness 10.0 mm, Wavelength 2325 nm | 75.2 % @Thickness 0.394 in, Wavelength 2325 nm |
| 91 % @Thickness 25.0 mm, Wavelength 1970 nm | 91 % @Thickness 0.984 in, Wavelength 1970 nm |
| 96.3 % @Thickness 10.0 mm, Wavelength 1970 nm | 96.3 % @Thickness 0.394 in, Wavelength 1970 nm |
| 98.7 % @Thickness 25.0 mm, Wavelength 1530 nm | 98.7 % @Thickness 0.984 in, Wavelength 1530 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1530 nm | 99.5 % @Thickness 0.394 in, Wavelength 1530 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 1060 nm | 99.6 % @Thickness 0.984 in, Wavelength 1060 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1060 nm | 99.8 % @Thickness 0.394 in, Wavelength 1060 nm |
UV Transmittance | 1.0 % @Thickness 25.0 mm, Wavelength 390 nm | 1.0 % @Thickness 0.984 in, Wavelength 390 nm |
| 2.6 % @Thickness 10.0 mm, Wavelength 380 nm | 2.6 % @Thickness 0.394 in, Wavelength 380 nm |
| 4.0 % @Thickness 25.0 mm, Wavelength 400 nm | 4.0 % @Thickness 0.984 in, Wavelength 400 nm |
| 9.0 % @Thickness 25.0 mm, Wavelength 405 nm | 9.0 % @Thickness 0.984 in, Wavelength 405 nm |
| 12.3 % @Thickness 10.0 mm, Wavelength 390 nm | 12.3 % @Thickness 0.394 in, Wavelength 390 nm |
| 29.2 % @Thickness 10.0 mm, Wavelength 400 nm | 29.2 % @Thickness 0.394 in, Wavelength 400 nm |
| 38.2 % @Thickness 10.0 mm, Wavelength 405 nm | 38.2 % @Thickness 0.394 in, Wavelength 405 nm |
|
Descriptive Properties |
---|
Climatic resistance | 2 |
Phosphate resistance | 4.3 |
Stress optical coefficient | 1.86 |