Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.80 g/cc | 1.80 g/cc |
Bulk Density | 1.80 g/cc | 0.0650 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 50 - 60 | 50 - 60 |
Hardness, Vickers | 55 - 70 | 55 - 70 |
Tensile Strength at Break | >= 140 MPa | >= 20300 psi |
| 80.0 MPa @Temperature 300 °C | 11600 psi @Temperature 572 °F |
| 125 MPa @Temperature 200 °C | 18100 psi @Temperature 392 °F |
| 150 MPa @Temperature 100 °C | 21800 psi @Temperature 212 °F |
| 160 MPa @Temperature 20.0 °C | 23200 psi @Temperature 68.0 °F |
Tensile Strength, Ultimate | 154 MPa @Temperature -196 °C | 22300 psi @Temperature -321 °F |
Tensile Strength, Yield | >= 95.0 MPa @Strain 0.2 % | >= 13800 psi @Strain 0.2 % |
| 50.0 MPa @Strain 0.2 %, Temperature 300 °C | 7250 psi @Strain 0.2 %, Temperature 572 °F |
| 75.0 MPa @Strain 0.2 %, Temperature 200 °C | 10900 psi @Strain 0.2 %, Temperature 392 °F |
| 80.0 MPa @Strain 0.2 %, Temperature 100 °C | 11600 psi @Strain 0.2 %, Temperature 212 °F |
| 110 MPa @Strain 0.2 %, Temperature 20.0 °C | 16000 psi @Strain 0.2 %, Temperature 68.0 °F |
Elongation at Break | >= 3.0 % | >= 3.0 % |
| 0.50 % @Temperature -196 °C | 0.50 % @Temperature -321 °F |
| 3.0 % @Temperature 22.0 °C | 3.0 % @Temperature 71.6 °F |
| 15 % @Temperature 100 °C | 15 % @Temperature 212 °F |
| 25 % @Temperature 200 °C | 25 % @Temperature 392 °F |
| 50 % @Temperature 300 °C | 50 % @Temperature 572 °F |
Creep Strength | 15.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 2180 psi @Temperature 482 °F, Time 1000 hour |
| 20.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 2900 psi @Temperature 482 °F, Time 1000 hour |
| 24.0 MPa @Temperature 250 °C, Time 360000 sec | 3480 psi @Temperature 482 °F, Time 100 hour |
| 26.0 MPa @Temperature 250 °C, Time 360000 sec | 3770 psi @Temperature 482 °F, Time 100 hour |
| 26.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 3770 psi @Temperature 482 °F, Time 1000 hour |
| 28.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 4060 psi @Temperature 482 °F, Time 1000 hour |
| 31.0 MPa @Temperature 250 °C, Time 360000 sec | 4500 psi @Temperature 482 °F, Time 100 hour |
| 32.0 MPa @Temperature 250 °C, Time 36000 sec | 4640 psi @Temperature 482 °F, Time 10.0 hour |
| 35.0 MPa @Temperature 200 °C, Time 3.60e+6 sec | 5080 psi @Temperature 392 °F, Time 1000 hour |
| 35.0 MPa @Temperature 250 °C, Time 36000 sec | 5080 psi @Temperature 482 °F, Time 10.0 hour |
| 47.0 MPa @Temperature 200 °C, Time 3.60e+6 sec | 6820 psi @Temperature 392 °F, Time 1000 hour |
| 51.0 MPa @Temperature 200 °C, Time 360000 sec | 7400 psi @Temperature 392 °F, Time 100 hour |
| 55.0 MPa @Temperature 200 °C, Time 3.60e+6 sec | 7980 psi @Temperature 392 °F, Time 1000 hour |
| 65.0 MPa @Temperature 200 °C, Time 360000 sec | 9430 psi @Temperature 392 °F, Time 100 hour |
Modulus of Elasticity | 44.0 GPa | 6380 ksi |
Compressive Yield Strength | 85.0 - 120 MPa @Strain 0.2 % | 12300 - 17400 psi @Strain 0.2 % |
Compressive Strength | 275 - 340 MPa | 39900 - 49300 psi |
Ultimate Bearing Strength | 395 MPa | 57300 psi |
Bearing Yield Strength | 275 MPa | 39900 psi |
Poissons Ratio | 0.33 | 0.33 |
Fatigue Strength | 46.0 MPa @# of Cycles 1.00e+7 , Temperature 300 °C | 6670 psi @# of Cycles 1.00e+7 , Temperature 572 °F |
| 47.0 MPa @# of Cycles 1.00e+6 , Temperature 300 °C | 6820 psi @# of Cycles 1.00e+6 , Temperature 572 °F |
| 48.0 MPa @# of Cycles 1.00e+7 , Temperature 250 °C | 6960 psi @# of Cycles 1.00e+7 , Temperature 482 °F |
| 50.0 MPa @# of Cycles 1.00e+6 , Temperature 250 °C | 7250 psi @# of Cycles 1.00e+6 , Temperature 482 °F |
| 50.0 MPa @# of Cycles 100000 , Temperature 300 °C | 7250 psi @# of Cycles 100000 , Temperature 572 °F |
| 54.0 MPa @# of Cycles 1.00e+7 , Temperature 200 °C | 7830 psi @# of Cycles 1.00e+7 , Temperature 392 °F |
| 55.0 MPa @# of Cycles 1.00e+6 , Temperature 200 °C | 7980 psi @# of Cycles 1.00e+6 , Temperature 392 °F |
| 55.0 MPa @# of Cycles 100000 , Temperature 250 °C | 7980 psi @# of Cycles 100000 , Temperature 482 °F |
| 59.0 MPa @# of Cycles 1.00e+7 , Temperature 150 °C | 8560 psi @# of Cycles 1.00e+7 , Temperature 302 °F |
| 60.0 MPa @# of Cycles 1.00e+6 , Temperature 150 °C | 8700 psi @# of Cycles 1.00e+6 , Temperature 302 °F |
| 67.0 MPa @# of Cycles 100000 , Temperature 200 °C | 9720 psi @# of Cycles 100000 , Temperature 392 °F |
| 70.0 MPa @# of Cycles 100000 , Temperature 150 °C | 10200 psi @# of Cycles 100000 , Temperature 302 °F |
| 78.0 MPa @# of Cycles 1.00e+7 , Temperature 20.0 °C | 11300 psi @# of Cycles 1.00e+7 , Temperature 68.0 °F |
| 80.0 MPa @# of Cycles 1.00e+6 , Temperature 20.0 °C | 11600 psi @# of Cycles 1.00e+6 , Temperature 68.0 °F |
| 15.0 MPa @# of Cycles 1.00e+7 | 2180 psi @# of Cycles 1.00e+7 |
| 20.0 MPa @# of Cycles 1.00e+6 | 2900 psi @# of Cycles 1.00e+6 |
| 28.0 MPa @# of Cycles 1.00e+7 | 4060 psi @# of Cycles 1.00e+7 |
| 30.0 MPa @# of Cycles 1.00e+6 | 4350 psi @# of Cycles 1.00e+6 |
| 40.0 MPa @# of Cycles 100000 | 5800 psi @# of Cycles 100000 |
| 60.0 MPa @# of Cycles 100000 | 8700 psi @# of Cycles 100000 |
| 66.0 MPa @# of Cycles 1.00e+7 | 9570 psi @# of Cycles 1.00e+7 |
| 68.0 MPa @# of Cycles 1.00e+6 | 9860 psi @# of Cycles 1.00e+6 |
| 90.0 MPa @# of Cycles 100000 | 13100 psi @# of Cycles 100000 |
Shear Strength | 138 MPa | 20000 psi |
Impact Test | 0.700 - 2.00 J | 0.516 - 1.48 ft-lb |
| 6.10 - 7.40 J | 4.50 - 5.46 ft-lb |
| 0.500 J @Temperature -196 °C | 0.369 ft-lb @Temperature -321 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000630 ohm-cm | 0.00000630 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 26.8 µm/m-°C | 14.9 µin/in-°F |
Specific Heat Capacity | 1.04 J/g-°C | 0.249 BTU/lb-°F |
Thermal Conductivity | 100 W/m-K | 694 BTU-in/hr-ft²-°F |
Melting Point | 545 - 640 °C | 1010 - 1180 °F |
Solidus | 545 °C | 1010 °F |
Liquidus | 640 °C | 1180 °F |
Maximum Service Temperature, Air | 250 °C | 482 °F |
Shrinkage | 1.5 % | 1.5 % |
|
Component Elements Properties | Metric | English | Comments |
---|
Magnesium, Mg | 92 - 95.1 % | 92 - 95.1 % |
Rare Earths | 2.5 - 4.0 % | 2.5 - 4.0 % |
Zinc, Zn | 2.0 - 3.0 % | 2.0 - 3.0 % |
Zirconium, Zr | 0.40 - 1.0 % | 0.40 - 1.0 % |
|
Descriptive Properties |
---|
Corrosion rate | 270 mpy |
Damping Index | 1.89 |