Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.84 g/cc | 1.84 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 55 - 70 | 55 - 70 |
Hardness, Vickers | 60 - 80 | 60 - 80 |
Tensile Strength at Break | >= 200 MPa | >= 29000 psi |
| >= 75.0 MPa @Temperature 300 °C | >= 10900 psi @Temperature 572 °F |
| >= 150 MPa @Temperature 200 °C | >= 21800 psi @Temperature 392 °F |
| >= 200 MPa @Temperature 100 °C | >= 29000 psi @Temperature 212 °F |
| 218 MPa @Temperature 20.0 °C | 31600 psi @Temperature 68.0 °F |
| 245 MPa @Temperature -196 °C | 35500 psi @Temperature -321 °F |
| 208 - 234 MPa @Thickness 19.0 - 32.0 mm | 30200 - 33900 psi @Thickness 0.748 - 1.26 in |
| 207 - 239 MPa @Thickness 32.0 - 45.0 mm | 30000 - 34700 psi @Thickness 1.26 - 1.77 in |
| 214 - 237 MPa @Thickness 5.00 mm | 31000 - 34400 psi @Thickness 0.197 in |
| 204 - 250 MPa @Thickness 15.0 mm | 29600 - 36300 psi @Thickness 0.591 in |
| 204 - 251 MPa @Thickness 10.0 mm | 29600 - 36400 psi @Thickness 0.394 in |
| 216 - 253 MPa @Thickness 19.0 mm | 31300 - 36700 psi @Thickness 0.748 in |
Tensile Strength, Yield | >= 135 MPa @Strain 0.2 % | >= 19600 psi @Strain 0.2 % |
| 148 MPa @Strain 0.2 % | 21500 psi @Strain 0.2 % |
| 60.0 MPa @Strain 0.2 %, Temperature 300 °C | 8700 psi @Strain 0.2 %, Temperature 572 °F |
| 115 MPa @Strain 0.2 %, Temperature 200 °C | 16700 psi @Strain 0.2 %, Temperature 392 °F |
| 135 MPa @Strain 0.2 %, Temperature 100 °C | 19600 psi @Strain 0.2 %, Temperature 212 °F |
| 142 MPa @Strain 0.2 %, Thickness 19.0 - 32.0 mm | 20600 psi @Strain 0.2 %, Thickness 0.748 - 1.26 in |
| 139 - 146 MPa @Strain 0.2 %, Thickness 32.0 - 45.0 mm | 20200 - 21200 psi @Strain 0.2 %, Thickness 1.26 - 1.77 in |
| 139 - 153 MPa @Strain 0.2 %, Thickness 5.00 mm | 20200 - 22200 psi @Strain 0.2 %, Thickness 0.197 in |
| 133 - 165 MPa @Strain 0.2 %, Thickness 15.0 mm | 19300 - 23900 psi @Strain 0.2 %, Thickness 0.591 in |
| 139 - 162 MPa @Strain 0.2 %, Thickness 19.0 mm | 20200 - 23500 psi @Strain 0.2 %, Thickness 0.748 in |
| 146 - 188 MPa @Strain 0.2 %, Thickness 10.0 mm | 21200 - 27300 psi @Strain 0.2 %, Thickness 0.394 in |
Elongation at Break | >= 3.0 % | >= 3.0 % |
| 0.50 % @Temperature -196 °C | 0.50 % @Temperature -321 °F |
| 4.5 % @Temperature 22.0 °C | 4.5 % @Temperature 71.6 °F |
| 5.0 % @Temperature 100 °C | 5.0 % @Temperature 212 °F |
| 25 % @Temperature 200 °C | 25 % @Temperature 392 °F |
| 40 % @Temperature 300 °C | 40 % @Temperature 572 °F |
| 4.0 - 7.0 % @Thickness 5.00 mm | 4.0 - 7.0 % @Thickness 0.197 in |
| 3.0 - 8.0 % @Thickness 32.0 - 45.0 mm | 3.0 - 8.0 % @Thickness 1.26 - 1.77 in |
| 2.0 - 9.5 % @Thickness 10.0 mm | 2.0 - 9.5 % @Thickness 0.394 in |
| 3.5 - 9.0 % @Thickness 15.0 mm | 3.5 - 9.0 % @Thickness 0.591 in |
| 4.0 - 11 % @Thickness 19.0 mm | 4.0 - 11 % @Thickness 0.748 in |
| 7.0 - 9.0 % @Thickness 19.0 - 32.0 mm | 7.0 - 9.0 % @Thickness 0.748 - 1.26 in |
Creep Strength | 0.000 MPa @Temperature 100 °C, Time 360000 sec | 0.000 psi @Temperature 212 °F, Time 100 hour |
| 69.0 MPa @Temperature 150 °C, Time 3.60e+6 sec | 10000 psi @Temperature 302 °F, Time 1000 hour |
| 77.0 MPa @Temperature 150 °C, Time 360000 sec | 11200 psi @Temperature 302 °F, Time 100 hour |
| 82.0 MPa @Temperature 150 °C, Time 3.60e+6 sec | 11900 psi @Temperature 302 °F, Time 1000 hour |
| 85.0 MPa @Temperature 150 °C, Time 360000 sec | 12300 psi @Temperature 302 °F, Time 100 hour |
| 91.0 MPa @Temperature 150 °C, Time 3.60e+6 sec | 13200 psi @Temperature 302 °F, Time 1000 hour |
| 93.0 MPa @Temperature 150 °C, Time 18000 sec | 13500 psi @Temperature 302 °F, Time 5.00 hour |
| 95.0 MPa @Temperature 150 °C, Time 360000 sec | 13800 psi @Temperature 302 °F, Time 100 hour |
| 98.0 MPa @Temperature 150 °C, Time 18000 sec | 14200 psi @Temperature 302 °F, Time 5.00 hour |
| 98.0 MPa @Temperature 100 °C, Time 18000 sec | 14200 psi @Temperature 212 °F, Time 5.00 hour |
| 99.0 MPa @Temperature 150 °C, Time 3.60e+6 sec | 14400 psi @Temperature 302 °F, Time 1000 hour |
| 100 MPa @Temperature 150 °C, Time 3.60e+6 sec | 14500 psi @Temperature 302 °F, Time 1000 hour |
| 102 MPa @Temperature 150 °C, Time 1.80e+6 sec | 14800 psi @Temperature 302 °F, Time 500 hour |
| 102 MPa @Temperature 150 °C, Time 360000 sec | 14800 psi @Temperature 302 °F, Time 100 hour |
| 103 MPa @Temperature 100 °C, Time 3.60e+6 sec | 14900 psi @Temperature 212 °F, Time 1000 hour |
| 103 MPa @Temperature 150 °C, Time 18000 sec | 14900 psi @Temperature 302 °F, Time 5.00 hour |
| 108 MPa @Temperature 150 °C, Time 36000 sec | 15700 psi @Temperature 302 °F, Time 10.0 hour |
| 108 MPa @Temperature 150 °C, Time 360000 sec | 15700 psi @Temperature 302 °F, Time 100 hour |
| 111 MPa @Temperature 100 °C, Time 18000 sec | 16100 psi @Temperature 212 °F, Time 5.00 hour |
| 111 MPa @Temperature 100 °C, Time 360000 sec | 16100 psi @Temperature 212 °F, Time 100 hour |
| 117 MPa @Temperature 100 °C, Time 18000 sec | 17000 psi @Temperature 212 °F, Time 5.00 hour |
| 117 MPa @Temperature 100 °C, Time 3.60e+6 sec | 17000 psi @Temperature 212 °F, Time 1000 hour |
| 118 MPa @Temperature 100 °C, Time 360000 sec | 17100 psi @Temperature 212 °F, Time 100 hour |
| 119 MPa @Temperature 100 °C, Time 18000 sec | 17300 psi @Temperature 212 °F, Time 5.00 hour |
Modulus of Elasticity | 44.1 GPa | 6400 ksi |
Compressive Yield Strength | 130 - 150 MPa @Strain 0.2 % | 18900 - 21800 psi @Strain 0.2 % |
Compressive Strength | 330 - 365 MPa | 47900 - 52900 psi |
Poissons Ratio | 0.35 | 0.35 |
Fatigue Strength | 60.0 MPa @# of Cycles 1.00e+7 , Temperature 200 °C | 8700 psi @# of Cycles 1.00e+7 , Temperature 392 °F |
| 65.0 MPa @# of Cycles 1.00e+7 , Temperature 150 °C | 9430 psi @# of Cycles 1.00e+7 , Temperature 302 °F |
| 70.0 MPa @# of Cycles 1.00e+6 , Temperature 200 °C | 10200 psi @# of Cycles 1.00e+6 , Temperature 392 °F |
| 80.0 MPa @# of Cycles 1.00e+6 , Temperature 150 °C | 11600 psi @# of Cycles 1.00e+6 , Temperature 302 °F |
| 85.0 MPa @# of Cycles 100000 , Temperature 200 °C | 12300 psi @# of Cycles 100000 , Temperature 392 °F |
| 90.0 MPa @# of Cycles 1.00e+7 , Temperature 20.0 °C | 13100 psi @# of Cycles 1.00e+7 , Temperature 68.0 °F |
| 92.0 MPa @# of Cycles 1.00e+6 , Temperature 20.0 °C | 13300 psi @# of Cycles 1.00e+6 , Temperature 68.0 °F |
| 95.0 MPa @# of Cycles 100000 , Temperature 150 °C | 13800 psi @# of Cycles 100000 , Temperature 302 °F |
| 105 MPa @# of Cycles 100000 , Temperature 20.0 °C | 15200 psi @# of Cycles 100000 , Temperature 68.0 °F |
| 50.0 MPa @# of Cycles 1.00e+7 | 7250 psi @# of Cycles 1.00e+7 |
| 54.0 MPa @# of Cycles 1.00e+6 | 7830 psi @# of Cycles 1.00e+6 |
| 76.0 MPa @# of Cycles 100000 | 11000 psi @# of Cycles 100000 |
| 88.0 MPa @# of Cycles 1.00e+7 | 12800 psi @# of Cycles 1.00e+7 |
| 90.0 MPa @# of Cycles 1.00e+6 | 13100 psi @# of Cycles 1.00e+6 |
| 100 MPa @# of Cycles 1.00e+7 | 14500 psi @# of Cycles 1.00e+7 |
| 102 MPa @# of Cycles 1.00e+6 | 14800 psi @# of Cycles 1.00e+6 |
| 105 MPa @# of Cycles 100000 | 15200 psi @# of Cycles 100000 |
| 121 MPa @# of Cycles 100000 | 17500 psi @# of Cycles 100000 |
Fracture Toughness | 15.1 - 16.3 MPa-m½ | 13.7 - 14.8 ksi-in½ |
Shear Strength | 138 MPa | 20000 psi |
Impact Test | 0.700 J @Temperature -196 °C | 0.516 ft-lb @Temperature -321 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000680 ohm-cm | 0.00000680 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 27.1 µm/m-°C | 15.1 µin/in-°F |
Specific Heat Capacity | 0.960 J/g-°C | 0.229 BTU/lb-°F |
Thermal Conductivity | 109 W/m-K | 756 BTU-in/hr-ft²-°F |
Melting Point | 510 - 640 °C | 950 - 1180 °F |
Solidus | 510 °C | 950 °F |
Liquidus | 640 °C | 1180 °F |
Maximum Service Temperature, Air | 150 °C | 302 °F |
Shrinkage | 1.3 % | 1.3 % |
|
Component Elements Properties | Metric | English | Comments |
---|
Magnesium, Mg | 92.3 - 95.3 % | 92.3 - 95.3 % |
Rare Earths | 0.80 - 1.7 % | 0.80 - 1.7 % |
Zinc, Zn | 3.5 - 5.0 % | 3.5 - 5.0 % |
Zirconium, Zr | 0.40 - 1.0 % | 0.40 - 1.0 % |
|
Descriptive Properties |
---|
Corrosion rate | 320-480 mpy |
Damping Index | 1 |