MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Styrene Acrylonitrile (SAN), Molded
Categories: Polymer; Thermoplastic; SAN Polymer; Styrene Acrylonitrile (SAN), Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Styrene Acrylonitrile (SAN), Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.901 - 1.36 g/cc0.0326 - 0.0491 lb/in³Average value: 1.07 g/cc Grade Count:86
Water Absorption 0.200 - 0.300 %0.200 - 0.300 %Average value: 0.275 % Grade Count:4
Moisture Absorption at Equilibrium 0.200 - 0.300 %0.200 - 0.300 %Average value: 0.267 % Grade Count:6
Linear Mold Shrinkage 0.00200 - 0.00700 cm/cm0.00200 - 0.00700 in/inAverage value: 0.00421 cm/cm Grade Count:47
Melt Flow 0.900 - 120 g/10 min0.900 - 120 g/10 minAverage value: 21.5 g/10 min Grade Count:87
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 67.0 - 12067.0 - 120Average value: 84.1 Grade Count:21
Hardness, Rockwell R 77.0 - 12777.0 - 127Average value: 113 Grade Count:18
Ball Indentation Hardness 155 - 175 MPa22500 - 25400 psiAverage value: 162 MPa Grade Count:10
Tensile Strength, Ultimate 16.6 - 113 MPa2410 - 16400 psiAverage value: 68.0 MPa Grade Count:61
 104 - 104 MPa
@Temperature -40.0 - -40.0 °C
15100 - 15100 psi
@Temperature -40.0 - -40.0 °F
Average value: 104 MPa Grade Count:1
Tensile Strength, Yield 25.8 - 85.5 MPa3740 - 12400 psiAverage value: 66.1 MPa Grade Count:48
 32.0 - 32.0 MPa
@Temperature 80.0 - 80.0 °C
4640 - 4640 psi
@Temperature 176 - 176 °F
Average value: 32.0 MPa Grade Count:1
Elongation at Break 1.50 - 900 %1.50 - 900 %Average value: 24.7 % Grade Count:53
 3.70 - 3.70 %
@Temperature -40.0 - -40.0 °C
3.70 - 3.70 %
@Temperature -40.0 - -40.0 °F
Average value: 3.70 % Grade Count:1
Elongation at Yield 1.70 - 20.0 %1.70 - 20.0 %Average value: 6.31 % Grade Count:10
 2.10 - 2.10 %
@Temperature 80.0 - 80.0 °C
2.10 - 2.10 %
@Temperature 176 - 176 °F
Average value: 2.10 % Grade Count:1
Modulus of Elasticity 2.90 - 3.80 GPa421 - 551 ksiAverage value: 3.50 GPa Grade Count:28
Flexural Yield Strength 53.0 - 155 MPa7680 - 22500 psiAverage value: 105 MPa Grade Count:59
Flexural Modulus 0.848 - 6.85 GPa123 - 994 ksiAverage value: 3.22 GPa Grade Count:56
Izod Impact, Notched 0.101 - 5.69 J/cm0.190 - 10.7 ft-lb/inAverage value: 0.792 J/cm Grade Count:36
 0.26695 - 0.64068 J/cm
@Temperature -20.0 - 3.89 °C
0.50011 - 1.2003 ft-lb/in
@Temperature -4.00 - 39.0 °F
Average value: 0.411 J/cm Grade Count:3
Izod Impact, Unnotched 0.149 - 2.14 J/cm0.280 - 4.00 ft-lb/inAverage value: 0.564 J/cm Grade Count:5
Izod Impact, Notched (ISO) 1.70 - 18.9 kJ/m²0.809 - 8.98 ft-lb/in²Average value: 3.93 kJ/m² Grade Count:23
 2.00 - 6.006 kJ/m²
@Temperature -30.0 - 3.89 °C
0.952 - 2.858 ft-lb/in²
@Temperature -22.0 - 39.0 °F
Average value: 3.08 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) 15.0 - 20.6 kJ/m²7.14 - 9.79 ft-lb/in²Average value: 17.1 kJ/m² Grade Count:7
Charpy Impact Unnotched 1.00 - 2.90 J/cm²4.76 - 13.8 ft-lb/in²Average value: 1.80 J/cm² Grade Count:26
 1.50 - 2.10 J/cm²
@Temperature -30.0 - -30.0 °C
7.14 - 9.99 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 1.80 J/cm² Grade Count:12
Charpy Impact, Notched 0.100 - 0.600 J/cm²0.476 - 2.86 ft-lb/in²Average value: 0.209 J/cm² Grade Count:31
 0.150 - 0.150 J/cm²
@Temperature -30.0 - -30.0 °C
0.714 - 0.714 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 0.150 J/cm² Grade Count:1
Tensile Creep Modulus, 1 hour 3500 MPa508000 psiAverage value: 3500 MPa Grade Count:3
Tensile Creep Modulus, 1000 hours 2800 MPa406000 psiAverage value: 2800 MPa Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 - 1.00e+16 ohm-cm1.00e+13 - 1.00e+16 ohm-cmAverage value: 2.63e+15 ohm-cm Grade Count:16
Surface Resistance 1.00e+13 - 1.00e+15 ohm1.00e+13 - 1.00e+15 ohmAverage value: 8.74e+14 ohm Grade Count:15
Dielectric Constant 2.70 - 3.102.70 - 3.10Average value: 2.97 Grade Count:6
Dielectric Strength 30.0 - 34.0 kV/mm762 - 864 kV/inAverage value: 31.3 kV/mm Grade Count:3
Dissipation Factor 0.00400 - 0.008000.00400 - 0.00800Average value: 0.00583 Grade Count:6
Arc Resistance 120 - 180 sec120 - 180 secAverage value: 150 sec Grade Count:3
Comparative Tracking Index 400 - 600 V400 - 600 VAverage value: 500 V Grade Count:6
Hot Wire Ignition, HWI 15.0 - 30.0 sec15.0 - 30.0 secAverage value: 22.5 sec Grade Count:3
High Amp Arc Ignition, HAI 120 arcs120 arcsAverage value: 120 arcs Grade Count:3
High Voltage Arc-Tracking Rate, HVTR 10.0 mm/min0.394 in/minAverage value: 10.0 mm/min Grade Count:3
 
Thermal PropertiesMetricEnglishComments
CTE, linear 36.0 - 70.0 µm/m-°C20.0 - 38.9 µin/in-°FAverage value: 59.7 µm/m-°C Grade Count:30
Thermal Conductivity 0.113 - 0.195 W/m-K0.784 - 1.35 BTU-in/hr-ft²-°FAverage value: 0.164 W/m-K Grade Count:5
Deflection Temperature at 0.46 MPa (66 psi) 78.9 - 120 °C174 - 248 °FAverage value: 99.3 °C Grade Count:16
Deflection Temperature at 1.8 MPa (264 psi) 52.8 - 104 °C127 - 219 °FAverage value: 90.2 °C Grade Count:73
Vicat Softening Point 43.0 - 220 °C109 - 428 °FAverage value: 104 °C Grade Count:61
Glass Transition Temp, Tg 102 - 104 °C216 - 219 °FAverage value: 103 °C Grade Count:9
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:61
Oxygen Index 18.0 - 19.5 %18.0 - 19.5 %Average value: 18.7 % Grade Count:6
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.56 - 1.571.56 - 1.57Average value: 1.57 Grade Count:3
Haze 0.450 - 60.0 %0.450 - 60.0 %Average value: 8.14 % Grade Count:8
Gloss 66.0 - 92.0 %66.0 - 92.0 %Average value: 77.3 % Grade Count:3
Transmission, Visible 80.0 - 91.0 %80.0 - 91.0 %Average value: 89.3 % Grade Count:23
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 280 °C356 - 536 °FAverage value: 233 °C Grade Count:8
Nozzle Temperature 204 - 229 °C400 - 445 °FAverage value: 217 °C Grade Count:3
Melt Temperature 160 - 260 °C320 - 500 °FAverage value: 217 °C Grade Count:11
Mold Temperature 20.0 - 98.0 °C68.0 - 208 °FAverage value: 59.9 °C Grade Count:17
Injection Velocity 200 mm/sec7.87 in/secAverage value: 200 mm/sec Grade Count:3
Drying Temperature 71.1 - 85.0 °C160 - 185 °FAverage value: 79.1 °C Grade Count:16
Injection Pressure 4.90 - 137 MPa711 - 19800 psiAverage value: 79.8 MPa Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Polycarbonate, Molded
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced
Overview of materials for Styrene Acrylonitrile (SAN), Transparent
Overview of materials for Polystyrene, Molded, Unreinforced

O4920 / 78437

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.