MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polystyrene, Molded, Unreinforced
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Molded, Unreinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polystyrene". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.0130 - 1.18 g/cc0.000470 - 0.0426 lb/in³Average value: 0.984 g/cc Grade Count:142
Water Absorption 0.000 - 0.100 %0.000 - 0.100 %Average value: 0.0900 % Grade Count:35
Moisture Absorption at Equilibrium 0.100 %0.100 %Average value: 0.100 % Grade Count:20
Water Absorption at Saturation 0.100 %0.100 %Average value: 0.100 % Grade Count:5
Particle Size 2000 - 4000 µm2000 - 4000 µmAverage value: 3000 µm Grade Count:4
Linear Mold Shrinkage 0.00200 - 0.00800 cm/cm0.00200 - 0.00800 in/inAverage value: 0.00511 cm/cm Grade Count:65
Melt Flow 1.20 - 100 g/10 min1.20 - 100 g/10 minAverage value: 9.26 g/10 min Grade Count:161
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell L 48.0 - 82.048.0 - 82.0Average value: 67.6 Grade Count:16
Hardness, Rockwell M 35.0 - 80.035.0 - 80.0Average value: 72.8 Grade Count:20
Hardness, Rockwell R 71.0 - 12071.0 - 120Average value: 109 Grade Count:11
Ball Indentation Hardness 60.0 - 155 MPa8700 - 22500 psiAverage value: 134 MPa Grade Count:15
Tensile Strength, Ultimate 5.50 - 59.0 MPa798 - 8560 psiAverage value: 41.0 MPa Grade Count:106
Tensile Strength, Yield 4.22 - 59.0 MPa612 - 8560 psiAverage value: 32.3 MPa Grade Count:73
Elongation at Break 0.400 - 70.0 %0.400 - 70.0 %Average value: 13.7 % Grade Count:121
Elongation at Yield 1.40 - 40.0 %1.40 - 40.0 %Average value: 14.0 % Grade Count:5
Modulus of Elasticity 0.894 - 3.55 GPa130 - 515 ksiAverage value: 2.78 GPa Grade Count:80
Flexural Yield Strength 28.0 - 106 MPa4060 - 15400 psiAverage value: 70.9 MPa Grade Count:79
Flexural Modulus 0.894 - 3.60 GPa130 - 522 ksiAverage value: 2.68 GPa Grade Count:95
Poissons Ratio 0.2200.220Average value: 0.220 Grade Count:3
Shear Modulus 0.750 - 1.45 GPa109 - 210 ksiAverage value: 1.23 GPa Grade Count:7
Izod Impact, Notched 0.107 - 2.14 J/cm0.200 - 4.00 ft-lb/inAverage value: 0.455 J/cm Grade Count:81
 0.350 - 0.800 J/cm
@Temperature -40.0 - 0.000 °C
0.656 - 1.50 ft-lb/in
@Temperature -40.0 - 32.0 °F
Average value: 0.531 J/cm Grade Count:6
Izod Impact, Notched (ISO) 1.50 - 11.0 kJ/m²0.714 - 5.23 ft-lb/in²Average value: 4.58 kJ/m² Grade Count:25
 2.00 - 3.00 kJ/m²
@Temperature -30.0 - -30.0 °C
0.952 - 1.43 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 2.57 kJ/m² Grade Count:3
 1.50 - 8.00 kJ/m²
@Temperature -30.0 - -30.0 °C
0.714 - 3.81 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 2.57 kJ/m² Grade Count:6
 1.50 - 8.00 kJ/m²
@Thickness 4.00 - 4.00 mm
0.714 - 3.81 ft-lb/in²
@Thickness 0.157 - 0.157 in
Average value: 2.57 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) 5.00 - 25.0 kJ/m²2.38 - 11.9 ft-lb/in²Average value: 8.69 kJ/m² Grade Count:12
Charpy Impact Unnotched 0.700 J/cm² - NB3.33 ft-lb/in² - NBAverage value: 2.28 J/cm² Grade Count:38
 1.00 - 16.0 J/cm²
@Temperature -40.0 - -30.0 °C
4.76 - 76.1 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 7.75 J/cm² Grade Count:4
Charpy Impact, Notched 0.200 - 1.60 J/cm²0.952 - 7.61 ft-lb/in²Average value: 0.476 J/cm² Grade Count:31
 0.150 - 0.360 J/cm²
@Temperature -40.0 - -30.0 °C
0.714 - 1.71 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 0.255 J/cm² Grade Count:2
Tensile Creep Modulus, 1 hour 3100 - 3300 MPa450000 - 479000 psiAverage value: 3240 MPa Grade Count:7
Tensile Creep Modulus, 1000 hours 2200 - 2600 MPa319000 - 377000 psiAverage value: 2470 MPa Grade Count:9
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1e+05 - 1.00e+18 ohm-cm1e+05 - 1.00e+18 ohm-cmAverage value: 9.06e+16 ohm-cm Grade Count:37
Surface Resistance 10000 - 1.00e+16 ohm10000 - 1.00e+16 ohmAverage value: 5.70e+14 ohm Grade Count:42
Static Decay 0.0100 - 2.00 sec0.0100 - 2.00 secAverage value: 0.543 sec Grade Count:5
Dielectric Constant 2.00 - 2.702.00 - 2.70Average value: 2.48 Grade Count:32
Dielectric Strength 19.7 - 160 kV/mm500 - 4060 kV/inAverage value: 77.2 kV/mm Grade Count:30
Dissipation Factor 0.0000500 - 0.002000.0000500 - 0.00200Average value: 0.000208 Grade Count:19
Arc Resistance 120 - 180 sec120 - 180 secAverage value: 150 sec Grade Count:3
Comparative Tracking Index 250 - 600 V250 - 600 VAverage value: 418 V Grade Count:25
Hot Wire Ignition, HWI 15.0 - 30.0 sec15.0 - 30.0 secAverage value: 22.5 sec Grade Count:4
High Amp Arc Ignition, HAI 120 arcs120 arcsAverage value: 120 arcs Grade Count:4
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/min0.394 - 1.00 in/minAverage value: 15.8 mm/min Grade Count:4
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 - 90.0 µm/m-°C22.2 - 50.0 µin/in-°FAverage value: 75.2 µm/m-°C Grade Count:27
Thermal Conductivity 0.170 W/m-K1.18 BTU-in/hr-ft²-°FAverage value: 0.170 W/m-K Grade Count:12
Deflection Temperature at 0.46 MPa (66 psi) 70.0 - 108 °C158 - 226 °FAverage value: 87.7 °C Grade Count:31
Deflection Temperature at 1.8 MPa (264 psi) 62.0 - 98.0 °C144 - 208 °FAverage value: 81.3 °C Grade Count:112
Vicat Softening Point 70.0 - 108 °C158 - 226 °FAverage value: 95.0 °C Grade Count:143
Glass Transition Temp, Tg 83.0 - 100 °C181 - 212 °FAverage value: 90.5 °C Grade Count:6
Flammability, UL94 HB - V-0HB - V-0Grade Count:91
Flame Spread 26.0 - 35.0 mm/min1.02 - 1.38 in/minAverage value: 27.9 mm/min Grade Count:8
Oxygen Index 18.0 - 25.0 %18.0 - 25.0 %Average value: 19.6 % Grade Count:8
Glow Wire Test 650 - 850 °C1200 - 1560 °FAverage value: 670 °C Grade Count:14
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.59 - 1.591.59 - 1.59Average value: 1.59 Grade Count:7
Haze 0.350 - 88.0 %0.350 - 88.0 %Average value: 13.1 % Grade Count:7
Transmission, Visible 1.00 - 92.0 %1.00 - 92.0 %Average value: 86.1 % Grade Count:27
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 300 °C374 - 572 °FAverage value: 223 °C Grade Count:6
Melt Temperature 40.0 - 280 °C104 - 536 °FAverage value: 217 °C Grade Count:56
Mold Temperature 10.0 - 82.0 °C50.0 - 180 °FAverage value: 41.8 °C Grade Count:49
Injection Velocity 200 mm/sec7.87 in/secAverage value: 200 mm/sec Grade Count:3
Drying Temperature 60.0 - 85.0 °C140 - 185 °FAverage value: 72.0 °C Grade Count:23
Moisture Content 0.0300 - 0.250 %0.0300 - 0.250 %Average value: 0.148 % Grade Count:10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polycarbonate, Molded
Overview of materials for Polypropylene, Molded
Overview of materials for Polystyrene, Extrusion Grade
Overview of materials for High Density Polyethylene (HDPE), Injection Molded
Overview of materials for Polystyrene, Impact Modified

O4800 / 77775

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.