MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Master Bond UV15 One Component UV Curable Epoxy
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes:
  • Low viscosity
  • Exceptional thermal stability
  • Very low shrinkage upon cure
  • Cationic curing system
Product Description: Master Bond UV15 is a high strength, low viscosity, epoxy based UV curable system for bonding, sealing and coating. It is 100% reactive and does not contain any solvents or other volatiles. It is also completely free of any oxygen inhibition. UV15 will cure quickly and easily when exposed to a UV light source with a wavelength range between 320- 365 nm, with the optimum at 365 nm. The energy required is typically 20-40 milliwatts per cm². The rate of cure depends upon the distance of the light from the material being cured, the thickness of the section and the intensity of the light source. It typically cures in thicknesses of a few microns to 0.015-0.020 inches in 15-30 seconds or less. Epoxy based UVs are described as having a cationic curing reaction. This kind of system will have lower shrinkage (1-2%) and higher temperature resistance than the majority of UV systems, which cure by a free radical mechanism. UV15 has excellent resistance to a wide variety of chemicals including water, acids, bases, fuels and many solvents. It features superb physical strength characteristics and electrical insulation properties. UV15 has superior adhesion to a wide variety of substrates including plastics, glass and many metals. As is typical with UVs, it has excellent optical clarity and light transmission properties. It is important to note that UV15’s low viscosity allows it to be spin coated. Cationic systems, such as UV15, tend to have much higher temperature resistance than other UV type systems. Its glass transition temperature (Tg) with a straight UV cure is 90-95°C, and when post cured for 30 minutes at 125°C, the Tg is 125-130°C. This post cure also enhances UV15’s chemical resistance. The service temperature range for this system is -80°F to +350°F. It is widely used for a variety of applications in the optical, optoelectronic, aerospace and related industries.

Product Advantages:

  • One component system; no mixing needed
  • Very low viscosity, easily applied; readily spin coated
  • No oxygen inhibition while curing
  • Cationic curing system
  • Superior temperature resistance, especially when post cured with heat
  • Outstanding optical clarity; excellent light transmission
  • High bond strength; excellent adhesion to surface treated metals, glass and many plastics

Information provided by Master Bond Inc.

Vendors: Master Bond is a leading manufacturer of adhesives, sealants, coatings and potting compounds. Master Bond’s vast product line consists of over 3,000 epoxy, polyurethane, silicone, cyanoacrylate and latex adhesives that vary in viscosity, cure speed, strength, chemical resistance, electrical properties, etc. Our custom adhesives offer design flexibility and provide excellent bonding performance. Visit www.masterbond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Viscosity 115 - 350 cP115 - 350 cP
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D >= 75>= 75
Tensile Strength >= 41.4 MPa>= 6000 psi
Tensile Modulus 1.72 - 2.07 GPa250 - 300 ksi
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+14 ohm-cm>= 1.00e+14 ohm-cm
Dielectric Constant  2.96
@Frequency 1e+6 Hz,
Temperature 25.0 °C
2.96
@Frequency 1e+6 Hz,
Temperature 77.0 °F
 3.14
@Frequency 60 Hz,
Temperature 25.0 °C
3.14
@Frequency 60 Hz,
Temperature 77.0 °F
 3.52
@Frequency 1e+6 Hz,
Temperature 100 °C
3.52
@Frequency 1e+6 Hz,
Temperature 212 °F
 3.76
@Frequency 1e+6 Hz,
Temperature 150 °C
3.76
@Frequency 1e+6 Hz,
Temperature 302 °F
 3.91
@Frequency 60 Hz,
Temperature 100 °C
3.91
@Frequency 60 Hz,
Temperature 212 °F
 4.85
@Frequency 60 Hz,
Temperature 150 °C
4.85
@Frequency 60 Hz,
Temperature 302 °F
Dissipation Factor  0.0040
@Frequency 1e+6 Hz,
Temperature 25.0 °C
0.0040
@Frequency 1e+6 Hz,
Temperature 77.0 °F
 0.020
@Frequency 60 Hz,
Temperature 25.0 °C
0.020
@Frequency 60 Hz,
Temperature 77.0 °F
 0.023
@Frequency 60 Hz,
Temperature 150 °C
0.023
@Frequency 60 Hz,
Temperature 302 °F
 0.026
@Frequency 1e+6 Hz,
Temperature 100 °C
0.026
@Frequency 1e+6 Hz,
Temperature 212 °F
 0.030
@Frequency 60 Hz,
Temperature 100 °C
0.030
@Frequency 60 Hz,
Temperature 212 °F
 0.032
@Frequency 1e+6 Hz,
Temperature 150 °C
0.032
@Frequency 1e+6 Hz,
Temperature 302 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 50.0 - 55.0 µm/m-°C27.8 - 30.6 µin/in-°F
Maximum Service Temperature, Air 177 °C350 °F
Minimum Service Temperature, Air -62.2 °C-80.0 °F
Glass Transition Temp, Tg 90.0 - 95.0 °C194 - 203 °Fwithout post cure
 125 - 130 °C257 - 266 °Fwith post cure
Shrinkage 1.0 - 2.0 %1.0 - 2.0 %
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5171.517
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month
@Temperature <=23.9 °C
6.00 Month
@Temperature <=75.0 °F
in original, unopened containers

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Master Bond Supreme 10AOHT Thermally Conductive One Component Epoxy System
Master Bond Supreme 42HT-2 Toughened Epoxy Resists Thermal Cycling
Master Bond UV15-7SP4 Low Shrinkage, One Component, UV Curable System
Master Bond UV15FL One Component, High Strength, Flexible UV Curable Epoxy
Master Bond EP30LTE-LO Dimensionally Stable Low Outgassing Two Part Epoxy

PMASTM968 / 185561

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.