MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Envalior Durethan® DP 1801/30 H3.0 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled; Nylon 6, Glass Fiber Filled, Flame Retardant

Material Notes: PA 6, injection molding grade, 30% milled fibers, UL 94V-2 at 0.8 mm, max. temperature in glow wire test: 960 °C at 0,75 mm, "halogen-free", good heat-ageing resistance

Application Examples: Medical Appliance Housings

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc0.0506 lb/in³ISO 1183
Water Absorption at Saturation 5.9 %5.9 %IOS 62
Linear Mold Shrinkage, Flow 0.0035 cm/cm0.0035 in/in150x105x3; ISO 2577
 0.0055 cm/cm0.0055 in/in60x60x2; ISO 2577
Linear Mold Shrinkage, Transverse 0.0063 cm/cm0.0063 in/in60x60x2; ISO 2577
 0.0095 cm/cm0.0095 in/in150x105x3; ISO 2577
Melt Flow 27.4 g/10 min
@Load 5.00 kg,
Temperature 260 °C
27.4 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 194 MPa28100 psiISO 2093-1
Tensile Strength at Break 93.0 MPa13500 psi5 mm/min; ISO 527-1,-2
Tensile Strength, Yield 96.0 MPa13900 psi50 mm/min; ISO 527-1,-2
Elongation at Break 4.0 %4.0 %5 mm/min; ISO 527-1,-2
Elongation at Yield 2.4 %2.4 %50 mm/min; ISO 527-1,-2
Tensile Modulus 7.60 GPa1100 ksi1 mm/min; ISO 527-1,-2
Flexural Strength 150 MPa21800 psi2 mm/min; ISO 178-A
Flexural Yield Strength 170 MPa
@Strain 3.5 %
24700 psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 7.30 GPa1060 ksi2 mm/min; ISO 178-A
Flexural Strain at Break 3.9 %3.9 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)  <= 10.0 kJ/m²
@Temperature 23.0 °C
<= 4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
<= 4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
Izod Impact, Unnotched (ISO) 35.0 kJ/m²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact Unnotched 5.00 J/cm²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact, Notched  <= 1.00 J/cm²
@Temperature 23.0 °C
<= 4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
 <= 1.00 J/cm²
@Temperature -30.0 °C
<= 4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
 <= 1.00 J/cm²
@Temperature -40.0 °C
<= 4.76 ft-lb/in²
@Temperature -40.0 °F
ISO 180-1A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Strength 38.0 kV/mm
@Thickness 1.00 mm
965 kV/in
@Thickness 0.0394 in
IEC 60243-1
Comparative Tracking Index 550 V550 VSolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 82.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
45.6 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow 35.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
19.4 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point 222 °C432 °F10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 210 °C410 °FISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 175 °C347 °FISO 75-1,-2
Vicat Softening Point 212 °C
@Load 5.10 kg
414 °F
@Load 11.2 lb
120°C/h; ISO 306
Flammability, UL94 V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
Oxygen Index 30 %30 %Method A; ISO 4589-2
Glow Wire Ignition Temperature 775 °C
@Thickness 3.00 mm
1430 °F
@Thickness 0.118 in
Glow Wire Flammability Index 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
Shrinkage, MD  0.090 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.090 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Shrinkage Flow Direction 150x105x3; ISO 2577
 0.14 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.14 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Shrinkage Flow Direction; 60x60x2; ISO 2577
Shrinkage, TD  0.15 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.15 %
@Treatment Temp. 248 °F,
Time 4.00 hour
60x60x2; ISO 2577
 0.24 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.24 %
@Treatment Temp. 248 °F,
Time 4.00 hour
150x105x3; ISO 2577

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior Durethan® DP 1801/30 H3.0 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Conditioned
Celanese Nilit Nilamid B G6 FR HF 30% Glass Fiber Reinforced, Flame Retardant PA6
Envalior Akulon® K222-KGV4 PA6-GF20 FR(30), Dry, 20% Glass Filled, Heat Stabilized, Flame Retardant
Envalior Durethan® DP 1852/30 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Dry
Envalior Arnite® AV2 365 SN PET-30% Glass Reinforced (European Grade)

PLANW9579 / 208315

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.