MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Durethan® DP 1801/30 H3.0 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled; Nylon 6, Glass Fiber Filled, Flame Retardant

Material Notes: PA 6, injection molding grade, 30% milled fibers, UL 94V-2 at 0.8 mm, max. temperature in glow wire test: 960 °C at 0,75 mm, "halogen-free", good heat-ageing resistance

Application Examples: Medical Appliance Housings

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.40 g/ccISO 1183
Water Absorption at Saturation 5.9 %IOS 62
Linear Mold Shrinkage, Flow 0.0035 cm/cm150x105x3; ISO 2577
 0.0055 cm/cm60x60x2; ISO 2577
Linear Mold Shrinkage, Transverse 0.0063 cm/cm60x60x2; ISO 2577
 0.0095 cm/cm150x105x3; ISO 2577
Melt Flow 27.4 g/10 min
@Load 5.00 kg,
Temperature 260 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 194 MPaISO 2093-1
Tensile Strength at Break 93.0 MPa5 mm/min; ISO 527-1,-2
Tensile Strength, Yield 96.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break 4.0 %5 mm/min; ISO 527-1,-2
Elongation at Yield 2.4 %50 mm/min; ISO 527-1,-2
Tensile Modulus 7600 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 150 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 170 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 7300 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 3.9 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 35.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched 50.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact, Notched <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -40.0 °C
ISO 180-1A
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Strength 38.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Comparative Tracking Index 550 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 82.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 35.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point 222 °C10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 210 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 175 °CISO 75-1,-2
Vicat Softening Point 212 °C
@Load 5.10 kg
120°C/h; ISO 306
Flammability, UL94 V-2
@Thickness 0.750 mm
Oxygen Index 30 %Method A; ISO 4589-2
Glow Wire Ignition Temperature 775 °C
@Thickness 3.00 mm
Glow Wire Flammability Index 960 °C
@Thickness 3.00 mm
Shrinkage, MD 0.090 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction 150x105x3; ISO 2577
 0.14 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction; 60x60x2; ISO 2577
Shrinkage, TD 0.15 %
@Treatment Temp. 120 °C,
Time 14400 sec
60x60x2; ISO 2577
 0.24 %
@Treatment Temp. 120 °C,
Time 14400 sec
150x105x3; ISO 2577

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Durethan® DP 1801/30 H3.0 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Conditioned
Celanese Nilit Nilamid B G6 FR HF 30% Glass Fiber Reinforced, Flame Retardant PA6
Envalior Akulon® K222-KGV4 PA6-GF20 FR(30), Dry, 20% Glass Filled, Heat Stabilized, Flame Retardant
Envalior Durethan® DP 1852/30 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Flame Retardant, Dry
Envalior Arnite® AV2 365 SN PET-30% Glass Reinforced (European Grade)

PLANW9579 / 208315

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.