MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Huntsman IROGRAN® A 85 P 4380 TPU-Polyether
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Ether Grade

Material Notes: Introduction: IROGRAN A 85 P 4380 is a flame-retardant, halogen-free, thermoplastic polyether-polyurethane intended for extrusion and injection molding applications. Additional characteristics of the product are excellent microbial resistance, high low-temperature flexibility, especially suitable for cable jackets.

Performance Features:

  • Excellent hydrolysis resistance
  • High microbial resistance
  • Low-adhesion surfaces
  • Flame retardant
  • Halogen-free
  • Good melt flow
  • UL 94 classification V2
Applications:
  • Cables
  • Hoses
  • Profiles
  • Cable Bushings

Information provided by Huntsman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³ASTM D792
Linear Mold Shrinkage 0.0080 cm/cm0.0080 in/inASTM D995
Melt Flow 30 - 60 g/10 min30 - 60 g/10 minMelt Volume Rate (cm³/10 min)
Melt Index of Compound 50 g/10 min
@Load 21.6 kg,
Temperature 190 °C
50 g/10 min
@Load 47.6 lb,
Temperature 374 °F
cm3/10 min
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8787ASTM D2240
Hardness, Shore D 3636ASTM D2240
Tensile Strength at Break 35.0 MPa5080 psiDIN 53504
Elongation at Break 610 %610 %ASTM D412
100% Modulus 6.50 MPa
@Strain 100 %
943 psi
@Strain 100 %
DIN 53504
300% Modulus 10.0 MPa
@Strain 300 %
1450 psi
@Strain 300 %
DIN 53504
Rebound 42 %42 %Bayshore; ASTM D2632
Tear Strength 80.6 kN/m460 pliASTM D624
Abrasion 3535[mm3]; ISO 4649
Compression Set  25 %
@Temperature 23.0 °C,
Time 252000 sec
25 %
@Temperature 73.4 °F,
Time 70.0 hour
ASTM D395
 45 %
@Temperature 70.0 °C,
Time 86400 sec
45 %
@Temperature 158 °F,
Time 24.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 159 - 180 °C318 - 356 °FHuntsman/TMA
Flammability, UL94 V-2V-2Non-Halogen FR
 
Processing PropertiesMetricEnglishComments
Feed Temperature 25.0 - 40.0 °C77.0 - 104 °FExtrusion
Front Barrel Temperature 165 - 190 °C329 - 374 °FExtrusion
Nozzle Temperature 170 - 200 °C338 - 392 °FExtrusion
 180 - 200 °C356 - 392 °FInjection
Adapter Temperature 175 - 195 °C347 - 383 °FExtrusion
Die Temperature 175 - 200 °C347 - 392 °FExtrusion
Melt Temperature 170 - 195 °C338 - 383 °FInjection
Mold Temperature 20.0 - 70.0 °C68.0 - 158 °FInjection
 
Descriptive Properties
Heating Zone175-195°CInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 65 P 4324 N TPU-Polyether
Huntsman IROGRAN® A 85 P 4350 TPU-Polyether
Huntsman IROGRAN® A 75 P 4665N TPU-Polyether
Huntsman IROGRAN® A 78 P 4766 TPU-Polyether
Huntsman IROGRAN® A 85 P 4394 TPU-Polyether

PHU9928 / 150388

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.