MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Huntsman IROGRAN® A 85 P 4394 TPU-Polyether
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Ether Grade

Material Notes: Introduction: IROGRAN A 85 P 4394 is a high performance polyether based thermoplastic polyurethane intended for extrusion and injection molding applications. IROGRAN A 85 P 4394 is part of the HUNTSMAN technical extrusion product range and offers a specially designed, flexible material with a broad processing window particularly suitable for the preparation of tubing, cable jacketing and technical moldings.

Performance Features:

  • High tensile strength
  • Excellent wear performance
  • Excellent hydrolysis & microbial resistance
  • Good low temperature flexibility

Information provided by Huntsman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.12 g/cc0.0405 lb/in³ASTM D792
Linear Mold Shrinkage 0.0080 cm/cm0.0080 in/inASTM D995
Melt Flow 50 - 80 g/10 min50 - 80 g/10 minMelt Volume Rate (cm³/10 min)
Melt Index of Compound 55 g/10 min
@Load 21.6 kg,
Temperature 190 °C
55 g/10 min
@Load 47.6 lb,
Temperature 374 °F
cm3/10 min
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8585ASTM D2240
Hardness, Shore D 3636ASTM D2240
Tensile Strength at Break 45.0 MPa6530 psiDIN 53504
Elongation at Break 610 %610 %ASTM D412
100% Modulus 7.00 MPa
@Strain 100 %
1020 psi
@Strain 100 %
DIN 53504
300% Modulus 12.0 MPa
@Strain 300 %
1740 psi
@Strain 300 %
DIN 53504
Rebound 36 %36 %Bayshore; ASTM D2632
Tear Strength 101 kN/m574 pliASTM D624
Abrasion 2525[mm3]; ISO 4649
Compression Set  20 %
@Temperature 23.0 °C,
Time 252000 sec
20 %
@Temperature 73.4 °F,
Time 70.0 hour
ASTM D395
 40 %
@Temperature 70.0 °C,
Time 86400 sec
40 %
@Temperature 158 °F,
Time 24.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 150 - 170 °C302 - 338 °FHuntsman/TMA
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 90 %90 %transparent; thickness not reported
 
Processing PropertiesMetricEnglishComments
Feed Temperature 25.0 - 40.0 °C77.0 - 104 °FExtrusion
Front Barrel Temperature 160 - 200 °C320 - 392 °FExtrusion
Nozzle Temperature 200 - 210 °C392 - 410 °FInjection
Adapter Temperature 175 - 200 °C347 - 392 °FExtrusion
Die Temperature 175 - 205 °C347 - 401 °FExtrusion
Melt Temperature 190 - 205 °C374 - 401 °FInjection
Mold Temperature 20.0 - 70.0 °C68.0 - 158 °FInjection
 
Descriptive Properties
Heating Zone170-210°CInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 92 P 4637 TPU-Polyether
Huntsman IROGRAN® A 65 P 4324 N TPU-Polyether
Huntsman IROGRAN® A 86 E 4486 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 80 P 5039 TPU-Polyether
Huntsman IROGRAN® A 85 D 4968 Polyester-Based TPU-Injection Extrusion Grade

PHU9929 / 150389

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.