MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Pyrotek ISOMAG® 70 Structural Insulation
Categories: Ceramic; Oxide; Magnesium Oxide; Silicon Oxide

Material Notes: Isomag® 70 is magnesia silicate based formulation provides insulating properties similar to calcium silicate with good strength and dimensional stability up to 1000°C.

Applications

  • Torpedo cars
  • Ladles
  • Tundishes
  • Fume hoods
  • Heat shields
  • Aluminum furnaces
  • Troughs
  • Vacuum degassers

Advantages

  • Low heat losses at higher temperatures
  • Low shrinkage at temperature use limit
  • Highest strength of any high temperature insulating board
  • High temperature rating
  • Asbestos and ceramic fiber free
  • Non wetted by molten aluminum

Information provided by Pyrotek.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.202 g/cc0.04343 lb/in³
Open Porosity 53.5 %53.5 %
 
Mechanical PropertiesMetricEnglishComments
Elongation at Yield 1.5 %
@Temperature 500 °C
1.5 %
@Temperature 932 °F
at 6.9 MPA
Flexural Strength 13.1 MPa1900 psi
Compressive Strength 15.1 MPa2190 psi
 17.0 MPa
@Strain 5.0 %,
Temperature 500 °C
2470 psi
@Strain 5.0 %,
Temperature 932 °F
 18.0 MPa
@Strain 5.0 %,
Temperature 300 °C
2610 psi
@Strain 5.0 %,
Temperature 572 °F
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.230 W/m-K
@Temperature 195 °C
1.60 BTU-in/hr-ft²-°F
@Temperature 383 °F
 0.240 W/m-K
@Temperature 315 °C
1.67 BTU-in/hr-ft²-°F
@Temperature 599 °F
 0.310 W/m-K
@Temperature 600 °C
2.15 BTU-in/hr-ft²-°F
@Temperature 1110 °F
Maximum Service Temperature, Air 1000 °C1830 °FContinuous use
 1050 °C1920 °F
Shrinkage  1.64 %
@Temperature 1000 °C
1.64 %
@Temperature 1830 °F
Linear
 4.0 %
@Temperature 1000 °C
4.0 %
@Temperature 1830 °F
Thickness

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Pyrotek ISOMAG® 175 Structural Insulation Board
Pyrotek ISOMAG® 45 Thermal Insulation Board
Pyrotek B-3A REFRACTORY BOARD
Pyrotek NAD-1000 High Temperature Engineering Board
Pyrotek ISOFLOW Graphite Rings Graphite Rings for Billet Casting Molds

CPYRO079 / 1817

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.