MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Thermal Ceramics TR-19 Block Insulation
Categories: Ceramic

Material Notes: TR-19 Block is an asbestos-free insulation products, manufactured from vermiculite granules and high temperature bonding materials. Because of its low conductivity, TR-19 Block is an economical, energy saving insulation. It exhibits minimal shrinkage at its 1900°F (1040°C) temperature limit, and will not readily decompose even when exposed directly to flame or cryolite vapor conditions.

Features:

  • Low thermal conductivity
  • Block construction 36" x 12"
  • Good high temperature strength
  • Variety of thicknesses up to 7”
  • Resistant to cryolite vapors

    Curved Block

  • Designed for curved or circular equipment
  • TR-19 recommended for temperatures up to 1900°F

    Applications:

  • Side and end wall insulating material in carbon baking pits
  • Backup insulation in aluminum pot cells, reheat and pusher furnaces, copper reverberatory furnaces, and oil-fired water tube boilers

    Curved Block

  • Interior and exterior use on bustle pipes, hot air pipes, stacks and other curved or circular equipment
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.3685 g/cc0.01331 lb/in³at ambient temperature; ASTM C303
     0.3765 g/cc
    @Temperature 1040 °C
    0.01360 lb/in³
    @Temperature 1900 °F
    ASTM C303
    Loss On Ignition 10 %10 %
    Porosity 93 %93 %ASTM C493
     
    Mechanical PropertiesMetricEnglishComments
    Modulus of Rupture 0.000827 GPa0.120 ksiat ambient temperature; ASTM C203
     0.000614 GPa
    @Temperature 1040 °C
    0.0890 ksi
    @Temperature 1900 °F
    ASTM C203
    Compressive Strength 1.27 MPa183 psiat ambient temperature; ASTM C165
     0.5001 MPa
    @Temperature 1040 °C
    72.53 psi
    @Temperature 1900 °F
    ASTM C165
     
    Thermal PropertiesMetricEnglishComments
    Specific Heat Capacity 0.840 J/g-°C0.201 BTU/lb-°F
    Thermal Conductivity  0.110 W/m-K
    @Temperature 204 °C
    0.763 BTU-in/hr-ft²-°F
    @Temperature 399 °F
     0.120 W/m-K
    @Temperature 316 °C
    0.833 BTU-in/hr-ft²-°F
    @Temperature 601 °F
     0.120 W/m-K
    @Temperature 426 °C
    0.833 BTU-in/hr-ft²-°F
    @Temperature 799 °F
     0.130 W/m-K
    @Temperature 540 °C
    0.902 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
     0.140 W/m-K
    @Temperature 649 °C
    0.972 BTU-in/hr-ft²-°F
    @Temperature 1200 °F
     0.150 W/m-K
    @Temperature 746 °C
    1.04 BTU-in/hr-ft²-°F
    @Temperature 1370 °F
     0.160 W/m-K
    @Temperature 856 °C
    1.11 BTU-in/hr-ft²-°F
    @Temperature 1570 °F
    Maximum Service Temperature, Air 1040 °C1900 °FContinuous
    Shrinkage 2.23 %
    @Temperature 1040 °C
    2.23 %
    @Temperature 1900 °F
    Linear; ASTM C356
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 9.1 %9.1 %
    Alkalis 2.6 %2.6 %
    CaO 15 %15 %
    Fe2O3 6.8 %6.8 %
    MgO 13 %13 %
    Other 0.40 %0.40 %
    SiO2 40 %40 %
    TiO2 1.2 %1.2 %
     
    Descriptive Properties
    Sulfur Trioxide Content, %0.4

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Overview of materials for Aluminum Alloy
    Aluminum 5456-H116; 5456-H321
    Overview of materials for 1000 Series Aluminum
    Aluminum Weldalite 049-T8
    Aluminum Alloys, General

    CTHERM019 / 2339

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.