MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Nickel Tin Bronze, UNS C94700, Copper Casting Alloy
Categories: Metal; Nonferrous Metal; Copper Alloy; Copper Casting Alloy

Material Notes:

Casting methods recommended for this alloy: Centrifugal, Continuous, Investment, Permanent Mold, and Sand.

Applications: Valve stems and bodies, bearings, wear guides, shift forks, feeding mechanisms, circuit breaker parts, gears, piston cylinders, nozzles.

Classified under: Nickel-tin bronzes. ASTM B584; formerly ASTM B292-A

As cast values below are for sand casting

Key Words: Nickel tin bronze, ASTM B584; ASTM B292-A
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.84 g/ccEstimated
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 85500 kg
 1803000 kg
Tensile Strength, Ultimate 345 MPaas cast
 586 MPaheat treated
Tensile Strength, Yield 159 MPaas cast
 414 MPaheat treated
Elongation at Break 10 %heat treated
 35 %as cast
Tensile Modulus 15000 ksi
Machinability 20 %heat treated; UNS C36000 (free-cutting brass) = 100%
 30 %as cast; UNS C36000 (free-cutting brass) = 100%
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000140 ohm-cm12% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.9 µin/in-°F
@Temperature 20.0 - 200 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 31.2 BTU-in/hr-ft²-°F
Melting Point 1660 - 1880 °F
Solidus 1660 °F
Liquidus 1880 °F
 
Processing PropertiesOriginal ValueComments
Precipitation Temperature 580 °F
@Time 299 sec
Air
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 88 %
Nickel, Ni 5.0 %
Tin, Sn 5.0 %
Zinc, Zn 2.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
High-Leaded Tin Bronze, UNS C93900, Copper Casting Alloy
High-Leaded Tin Bronze, UNS C94300, Copper Casting Alloy
Leaded Nickel Tin Bronze, UNS C94800, Copper Casting Alloy
Leaded Phosphor Bronze, UNS C94400, Copper Casting Alloy
Medium Bronze, UNS C94500, Copper Casting Alloy

MC94700b1 / 11958

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.