MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Röhm Vu-Stat™ C37 Static Dissipative Acrylic Multipolymer Compound  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, General Purpose, Molded

Material Notes: Vu-Stat C-37 compound is a transparent, electro-static dissipative acrylic multipolymer compound with outstanding ESD properties and an excellent balance of mechanical, thermal and flow properties. Developed specifically for electronic parts that are sensitive to static discharge, Vu-Stat C-37 compound retains permanent static dissipative properties even after several washings. This product can be processed in all types of injection molding presses.

Information provided by Cyro Industries

Information Provided by Evonik CYRO. The former Evonik Methacrylates business has been sold to Röhm (Roehm) GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Melt Flow 7.9 g/10 min
@Load 5.00 kg,
Temperature 230 °C
7.9 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell L 4444ASTM D785
Tensile Strength, Yield 33.64 MPa4879 psiASTM D638
Elongation at Break 19 %19 %ASTM D638
Elongation at Yield 4.7 %4.7 %ASTM D638
Tensile Modulus 1.53 GPa222 ksiASTM D638
Izod Impact, Notched  0.747 J/cm
@Thickness 6.35 mm,
Temperature 23.0 °C
1.40 ft-lb/in
@Thickness 0.250 in,
Temperature 73.4 °F
ASTM D256
 0.801 J/cm
@Thickness 3.17 mm,
Temperature 0.000 °C
1.50 ft-lb/in
@Thickness 0.125 in,
Temperature 32.0 °F
ASTM D256
 0.801 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
1.50 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
ASTM D256
 0.801 J/cm
@Thickness 6.35 mm,
Temperature 0.000 °C
1.50 ft-lb/in
@Thickness 0.250 in,
Temperature 32.0 °F
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 8.90e+10 ohm-cm8.90e+10 ohm-cm12% RH; ASTM D257-78
 1.80e+11 ohm-cm1.80e+11 ohm-cmAfter 24 hours Cold Water Showering; ASTM D257-78
Surface Resistance 2.60e+9 ohm2.60e+9 ohm12% RH; ASTM EOS/ESD 511.11
 2.70e+9 ohm2.70e+9 ohmAfter 24 hours Cold Water Showering; ASTM FTM 101C
Static Decay 0.020 sec0.020 secAfter 24 hours Cold Water Showering; ASTM EOS/ESD 511.11
 0.030 sec0.030 secAt 23°C, 12% RH; ASTM FTM 101C
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C185 °FASTM D648
Vicat Softening Point 104 °C219 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 10.2 %10.2 %ASTM D1003
Gloss 113 %113 %At 60°; ASTM D1003
Transmission, Visible 77 %77 %ASTM D1003
 
Processing PropertiesMetricEnglishComments
Melt Temperature 204 - 246 °C400 - 475 °F
Mold Temperature 32.2 - 60.0 °C90.0 - 140 °F
Drying Temperature 82.2 °C180 °F3-4hrs
Injection Pressure 68.9 - 82.7 MPa10000 - 12000 psiHydraulic
Back Pressure <= 0.689 MPa<= 100 psi
Screw Speed 20 - 70 rpm20 - 70 rpm3.5:1 Compression

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Delrin Delrin® 500AL NC010 POM-S
Asahi Kasei DELPET™ 720V Acrylic (PMMA), Standard Grade
Asahi Kasei DELPET™ SRB100 Acrylic (PMMA), High Impact
LG Chemical HF-380 ABS, High Flow, High Impact
Trinseo Plexiglas® SG7 Acrylic

PCYRO52 / 29229

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.