MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Abatron AboCast 8110-6/AboCure 8110-1 Flexible Epoxy
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive, Flexible

Material Notes: This epoxy system can achieve flexibility and plasticity without sacrificing adhesive, electrical, structural, and other properties. This compound is a clear (unfilled) basic formulation. Its applications include: bonding, laminating, casting, embedding, electrical potting, impregnating, coating, etc. It can be supplied in several variations to modify viscosity, reaction rate, color, most physical and chemical properties, and with many fillers to meet most requirements.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Water Absorption 2.5 %
@Time 7200 sec
2.5 %
@Time 2.00 hour
boil; cured 2 hours @ 93°C
Viscosity 2000 cP2000 cP
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  75
@Temperature 75.0 °C
75
@Temperature 167 °F
cured 2 hrs. @ 93°C
 83
@Temperature 25.0 °C
83
@Temperature 77.0 °F
cured 2 hrs. @ 93°C
 87
@Temperature 0.000 °C
87
@Temperature 32.0 °F
cured 2 hrs. @ 93°C
 90
@Temperature -60.0 °C
90
@Temperature -76.0 °F
cured 2 hrs. @ 93°C
Tensile Strength, Ultimate 43.33 MPa6285 psicured 2 hours @ 93°C
 58.16 MPa8435 psicured 8 hours @ 93°C
Elongation at Break 11 %11 %cured 8 hours @ 93°C
 13 %13 %cured 2 hours @ 93°C
Shear Strength  12.2 MPa
@Temperature 75.0 °C
1770 psi
@Temperature 167 °F
Tensile, Al/Al lap joint; cured 2 hours @ 93°C
 28.9 MPa
@Temperature 0.000 °C
4190 psi
@Temperature 32.0 °F
Tensile, Al/Al lap joint; cured 2 hours @ 93°C
 41.9 MPa
@Temperature 25.0 °C
6080 psi
@Temperature 77.0 °F
Tensile, Al/Al lap joint; cured 2 hours @ 93°C
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  7.90e+7 ohm-cm
@Temperature 150 °C
7.90e+7 ohm-cm
@Temperature 302 °F
cured 2 hours @ 93°C
 7.70e+8 ohm-cm
@Temperature 112 °C
7.70e+8 ohm-cm
@Temperature 234 °F
cured 2 hours @ 93°C
 2.70e+9 ohm-cm
@Temperature 100 °C
2.70e+9 ohm-cm
@Temperature 212 °F
cured 2 hours @ 93°C
 9.40e+14 ohm-cm
@Temperature 25.0 °C
9.40e+14 ohm-cm
@Temperature 77.0 °F
cured 2 hours @ 93°C
 
Processing PropertiesMetricEnglishComments
Pot Life 22 min
@Temperature 25.0 °C
22 min
@Temperature 77.0 °F
200 g
Gel Time 6.00 min
@Temperature 93.0 °C
6.00 min
@Temperature 199 °F
10 g
 
Descriptive Properties
Parts by Weight (pbw)10.2AboCure 8110-1
 100AboCast 8110-6

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Epoxy Adhesive, Flexible
Abatron AboCast/AboCure 8110-2 Flexible Epoxy
Abatron AboCast 8110-7/AboCure 8110-1 Flexible Epoxy
Abatron AboCast 8110-2/AboCure 8110-1 Flexible Epoxy
3M Scotch-Weld™ TE100 Black Polyurethane Reactive Adhesive

PABC872 / 107856

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.