MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik 20C Strip Steel
Categories: Metal; Ferrous Metal; Special-Purpose Steel

Material Notes: Sandvik 15LM and 20C are characterized by good properties in respect of:
  • Fatigue strength and wear resistance
  • Hardness combined with ductility
  • Dimensional tolerances
  • Surface and edge finishes
  • Shape
  • The materials also have good blanking and forming properties with retaining shape of the parts after the blanking operation.

    Information provided by Sandvik

    ASTM 1095; EN 1.1274

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 7.85 g/cc
     
    Mechanical PropertiesOriginal ValueComments
    Tensile Strength, Ultimate 2100 MPad<0.125
     1600 MPa
    @Diameter 1.00 - 3.50 mm
     1650 MPa
    @Diameter 0.825 - 1.00 mm
     1700 MPa
    @Diameter 0.625 - 0.825 mm
     1750 MPa
    @Diameter 0.475 - 0.625 mm
     1800 MPa
    @Diameter 0.425 - 0.475 mm
     1850 MPa
    @Diameter 0.375 - 0.425 mm
     1900 MPa
    @Diameter 0.275 - 0.375 mm
     1950 MPa
    @Diameter 0.225 - 0.275 mm
     2000 MPa
    @Diameter 0.175 - 0.225 mm
     2050 MPa
    @Diameter 0.125 - 0.175 mm
    Tensile Strength, Yield 1500 MPa
    @Diameter 0.825 - 1.00 mm
     1550 MPa
    @Diameter 0.625 - 0.825 mm
     1600 MPa
    @Diameter 0.425 - 0.625 mm
     1650 MPa
    @Diameter 0.375 - 0.425 mm
     1700 MPa
    @Diameter 0.275 - 0.375 mm
     1750 MPa
    @Diameter 0.225 - 0.275 mm
     1800 MPa
    @Diameter 0.175 - 0.225 mm
     1850 MPa
    @Diameter 0.125 - 0.175 mm
     1450 MPa
    @Diameter 1.00 - 3.50 mm,
    Strain 2 %
     1900 MPa
    @Diameter <=0.125 mm,
    Strain 2 %
     
    Thermal PropertiesOriginal ValueComments
    CTE, linear 10.4 µm/m-°C
    @Temperature 20.0 - 100 °C
     11.6 µm/m-°C
    @Temperature 20.0 - 200 °C
     12.4 µm/m-°C
    @Temperature 20.0 - 300 °C
    Thermal Conductivity 49.0 W/m-K
    @Temperature 20.0 °C
     
    Component Elements PropertiesOriginal ValueComments
    Carbon, C 1.0 %
    Iron, Fe 98.3 %As Balance
    Manganese, Mn 0.45 %
    Silicon, Si 0.25 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Sandvik 20C Shock Absorber Strip Steel
    303 Stainless Steel, annealed
    21Cr-32Ni-Ti-Al IRON BASED 21Cr-32Ni-Ti-Al ALLOY FOR HEAT EXCHANGER SEAMLESS TUBES (NCF 800H TB)
    AISI 1017 Steel, cold drawn
    660 Stainless Steel (A286) cold drawn wire diameter of 5.61 mm, aged at 540°C (1000°F)

    NSANDV281 / 19175

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.