MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 13766 Isobutylene-Isoprene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 13766 is a 70 durometer black colored general purpose Butyl elastomer. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 715 A13 EA14 F17; 3 AA 715 B13 B33 EA14 F17; 4 AA 715 A13 B13 B33 EA14 F17; 5 AA 715 A13 B13 B33 EA14 F17; 2 BA 715 F17; 3 BA 715 A14 B13 F17; 4 BA 715 A14 F17; 5 BA 715 F17; 6 BA 715 B13; 8 BA 712 B13

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.16 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 71
 0.00
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 52
@Treatment Temp. 70.0 °C,
Time 605000 sec
Tri-Butyl Phosphate
 67
@Treatment Temp. 100 °C,
Time 252000 sec
SAE Phosphate Ester Fluid
 72
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 73
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 75
@Treatment Temp. 70.0 °C,
Time 605000 sec
Heat Aged
Tensile Strength 2090 psi
 1145.3 psi
@Treatment Temp. 70.0 °C,
Time 605000 sec
Tri-Butyl Phosphate
 1845.5 psi
@Treatment Temp. 100 °C,
Time 252000 sec
SAE Phosphate Ester Fluid
 2058.65 psi
@Treatment Temp. 70.0 °C,
Time 605000 sec
Heat Aged
 2090 psi
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 2094.2 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 350 %
 220.1 %
@Treatment Temp. 70.0 °C,
Time 605000 sec
Tri-Butyl Phosphate
 280 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 293.6 %
@Treatment Temp. 70.0 °C,
Time 605000 sec
Heat Aged
 324.1 %
@Treatment Temp. 100 °C,
Time 252000 sec
SAE Phosphate Ester Fluid
 339.8 %
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
100% Modulus 489 psi
Tear Strength 247 pliDie B
Compression Set 12.1 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Solid
 19.8 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Plied
 42.9 %
@Treatment Temp. 100 °C,
Time 79200 sec
Solid
 71.1 %
@Treatment Temp. 100 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -50.0 °F
Shrinkage 1.3 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 4.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, SAE Phosphate Ester Fluid
 19.8 %
@Treatment Temp. 70.0 °C,
Time 605000 sec
Volume, Tri-Butyl Phosphate
 
Descriptive Properties
ColorBlack
TR-10 Temperature-56.7°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL239 / 318449

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.