Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.16 g/cc | 1.16 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 71 | 71 |
| 0.00 @Treatment Temp. 100 °C, Time 252000 sec | 0.00 @Treatment Temp. 212 °F, Time 70.0 hour |
| 52 @Treatment Temp. 70.0 °C, Time 605000 sec | 52 @Treatment Temp. 158 °F, Time 168 hour |
| 67 @Treatment Temp. 100 °C, Time 252000 sec | 67 @Treatment Temp. 212 °F, Time 70.0 hour |
| 72 @Treatment Temp. 70.0 °C, Time 252000 sec | 72 @Treatment Temp. 158 °F, Time 70.0 hour |
| 73 @Treatment Temp. 100 °C, Time 252000 sec | 73 @Treatment Temp. 212 °F, Time 70.0 hour |
| 75 @Treatment Temp. 70.0 °C, Time 605000 sec | 75 @Treatment Temp. 158 °F, Time 168 hour |
Tensile Strength | 14.4 MPa | 2090 psi |
| 7.8966 MPa @Treatment Temp. 70.0 °C, Time 605000 sec | 1145.3 psi @Treatment Temp. 158 °F, Time 168 hour |
| 12.724 MPa @Treatment Temp. 100 °C, Time 252000 sec | 1845.5 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 14.1939 MPa @Treatment Temp. 70.0 °C, Time 605000 sec | 2058.65 psi @Treatment Temp. 158 °F, Time 168 hour |
| 14.4 MPa @Treatment Temp. 70.0 °C, Time 252000 sec | 2090 psi @Treatment Temp. 158 °F, Time 70.0 hour |
| 14.439 MPa @Treatment Temp. 100 °C, Time 252000 sec | 2094.2 psi @Treatment Temp. 212 °F, Time 70.0 hour |
Elongation, Ultimate | 350 % | 350 % |
| 220.1 % @Treatment Temp. 70.0 °C, Time 605000 sec | 220.1 % @Treatment Temp. 158 °F, Time 168 hour |
| 280 % @Treatment Temp. 100 °C, Time 252000 sec | 280 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 293.6 % @Treatment Temp. 70.0 °C, Time 605000 sec | 293.6 % @Treatment Temp. 158 °F, Time 168 hour |
| 324.1 % @Treatment Temp. 100 °C, Time 252000 sec | 324.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 339.8 % @Treatment Temp. 70.0 °C, Time 252000 sec | 339.8 % @Treatment Temp. 158 °F, Time 70.0 hour |
100% Modulus | 3.37 MPa | 489 psi |
Tear Strength | 43.3 kN/m | 247 pli |
Compression Set | 12.1 % @Treatment Temp. 70.0 °C, Time 79200 sec | 12.1 % @Treatment Temp. 158 °F, Time 22.0 hour |
| 19.8 % @Treatment Temp. 70.0 °C, Time 79200 sec | 19.8 % @Treatment Temp. 158 °F, Time 22.0 hour |
| 42.9 % @Treatment Temp. 100 °C, Time 79200 sec | 42.9 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 71.1 % @Treatment Temp. 100 °C, Time 79200 sec | 71.1 % @Treatment Temp. 212 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -45.6 °C | -50.0 °F |
Shrinkage | 1.3 % @Treatment Temp. 100 °C, Time 252000 sec | 1.3 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 4.4 % @Treatment Temp. 100 °C, Time 252000 sec | 4.4 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 19.8 % @Treatment Temp. 70.0 °C, Time 605000 sec | 19.8 % @Treatment Temp. 158 °F, Time 168 hour |
|
Descriptive Properties |
---|
Color | Black |
TR-10 Temperature | -56.7°C |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding