MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol STAT-RITE® S-1100 Static Dissipative TPU
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP

Material Notes: Description: Stat-Rite® S1100 is a static dissipative TPU alloy. Stat-Rite S-1100 utilizes the patented Stat-Rite inherently dissipative polymer (IDP) alloy system to provide clean, permanent ESD protection. Stat-Rite® IDP alloys provide consistent static dissipation even when extruded, injection molded or thermoformed into components.

Features:

  • Permanent static dissipative
  • Humidity insensitive
  • Ultra-clean: low off-gassing, low ionic contamination
  • Colorable
  • Durable: Can be used for years and years

Applications:

  • ESD and Cleanroom Tubing
  • ESD and Cleanroom Hose
  • Cleanroom Curtains
  • Conveyor ESD Wear Strip, Rollers
  • ESD and Cleanroom Film

Available in Americas, Europe, Middle East, Africa, India and Asia

Information provided by Lubrizol.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.16 g/cc1.16 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9090ASTM D2240
Hardness, Shore D 4747ASTM D2240
Tensile Strength at Break 26.0 MPa3770 psiASTM D412
Elongation at Break 450 %450 %ASTM D412
100% Modulus 8.00 MPa
@Strain 100 %
1160 psi
@Strain 100 %
ASTM D412
300% Modulus 15.0 MPa
@Strain 300 %
2180 psi
@Strain 300 %
ASTM D412
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 5.00e+9 ohm-cm5.00e+9 ohm-cmASTM D257
Surface Resistance 5.00e+8 ohm5.00e+8 ohm12% RH; ESD S11.11
Surface Resistivity per Square 5.00e+9 ohm5.00e+9 ohm50%; ASTM D257
Static Decay 0.010 sec0.010 sec12% RH (+5000 V to 50 V); FTMS-101C
 0.010 sec0.010 sec12% RH (-5000 V to -50 V); FTMS-101C
 0.10 sec0.10 secCharged Plate Monitor, 50% RH (+1000 V to 100 V)
 
Processing PropertiesMetricEnglishComments
Drying Temperature 105 °C221 °Fdehumidifying hopper
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hour
 
Descriptive Properties
ColorLight Blue, Transparent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol STAT-RITE® S-1107 Static Dissipative TPU
Lubrizol STAT-RITE® E-1150 Ether-Type Static Dissipative Polymer
Lubrizol STAT-RITE® E-1140 Ester-Type Static Dissipative Polymer
Lubrizol Stat-Rite® S-250 Static Control Polypropylene
Lubrizol Stat-Rite® SIS535 Static Control System

PNOVEON068a / 138281

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.