MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

AiResist 213 Cobalt Alloy (AR-213)
Categories: Metal; Nonferrous Metal; Cobalt Alloy

Material Notes: Resistant to hot corrosion; typical applications: sheets, tubing. Precipitation Hardening.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  315 MPa
@Temperature 870 °C
45700 psi
@Temperature 1600 °F
 485 MPa
@Temperature 760 °C
70300 psi
@Temperature 1400 °F
 960 MPa
@Temperature 650 °C
139000 psi
@Temperature 1200 °F
 1120 MPa
@Temperature 21.0 °C
162000 psi
@Temperature 69.8 °F
Tensile Strength, Yield  220 MPa
@Strain 0.2 %,
Temperature 870 °C
31900 psi
@Strain 0.2 %,
Temperature 1600 °F
 385 MPa
@Strain 0.2 %,
Temperature 760 °C
55800 psi
@Strain 0.2 %,
Temperature 1400 °F
 425 MPa
@Strain 0.2 %,
Temperature 650 °C
61600 psi
@Strain 0.2 %,
Temperature 1200 °F
 625 MPa
@Strain 0.2 %,
Temperature 21.0 °C
90600 psi
@Strain 0.2 %,
Temperature 69.8 °F
Elongation at Break  14 %
@Temperature 21.0 °C
14 %
@Temperature 69.8 °F
 28 %
@Temperature 650 °C
28 %
@Temperature 1200 °F
 47 %
@Temperature 760 °C
47 %
@Temperature 1400 °F
 55 %
@Temperature 870 °C
55 %
@Temperature 1600 °F
Rupture Strength  19.3 MPa
@Temperature 1090 °C,
Time 360000 sec
2800 psi
@Temperature 2000 °F,
Time 100 hour
 24.1 MPa
@Temperature 982 °C,
Time 3.60e+6 sec
3500 psi
@Temperature 1800 °F,
Time 1000 hour
 34.5 MPa
@Temperature 982 °C,
Time 360000 sec
5000 psi
@Temperature 1800 °F,
Time 100 hour
 89.6 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
13000 psi
@Temperature 1500 °F,
Time 1000 hour
 138 MPa
@Temperature 816 °C,
Time 360000 sec
20000 psi
@Temperature 1500 °F,
Time 100 hour
 448 MPa
@Temperature 649 °C,
Time 360000 sec
65000 psi
@Temperature 1200 °F,
Time 100 hour
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.5 %3.5 %
Carbon, C 0.18 %0.18 %
Chromium, Cr 19 %19 %
Cobalt, Co 66 %66 %
Tantalum, Ta 6.5 %6.5 %
Tungsten, W 4.7 %4.7 %
Yttrium, Y 0.10 %0.10 %
Zirconium, Zr 0.15 %0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Grade 18Ni (350) Maraging Steel nominal annealed properties
Arcam ASTM F-75 Cobalt Chrome Alloy
AK Steel 316L Austenitic Stainless steel
Sylvania SA201 Tungsten & Chrome Based Thermal Spray Powder
Overview of materials for Maraging Steel

NZ988 / 170617

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.