MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

EnviroBrass® (SeBiLOY®) II Lead-Free Casting Alloy, UNS C89520
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: The bismuth and selenium additions take the place of lead in this red brass. The melting and machining behavior make this alloy a plausible substitute for C83600 and C84400 in plumbing applications.

Small section size effect on mechanical properties of castings. Hot tearing at abrupt section changes is much reduced versus leaded red brasses.

Information from the Copper Development Association.

Key Words: ASTM B 30 and B 584
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.80 g/cc0.318 lb/in³estimated from C83600
Porosity 0.4 %0.4 %Minimal porosity
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  >= 68
@Load 500 kg
>= 68
@Load 1100 lb
Sand Cast
 73
@Load 500 kg
73
@Load 1100 lb
Typical, Sand Cast
Tensile Strength, Ultimate >= 176 MPa>= 25500 psiSand Cast
 215 MPa31200 psiTypical, Sand Cast
Tensile Strength, Yield  >= 121 MPa
@Strain 0.5 %
>= 17500 psi
@Strain 0.5 %
Sand Cast
 145 MPa
@Strain 0.5 %
21000 psi
@Strain 0.5 %
Typical, Sand Cast
Elongation at Break >= 6.0 %>= 6.0 %Sand Cast
 10 %10 %Typical, Sand Cast
Machinability 85 %85 %Based on C36000 at 100%
 
Thermal PropertiesMetricEnglishComments
Melting Point 809 - 1010 °C1490 - 1840 °Flong freezing range
Solidus 809 °C1490 °F
Liquidus 1010 °C1840 °F
Shrinkage 1.9 - 3.6 %1.9 - 3.6 %upon casting
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.005 %<= 0.005 %
Antimony, Sb <= 0.25 %<= 0.25 %
Bismuth, Bi 1.6 - 2.2 %1.6 - 2.2 %Bi:Se ratio > 2:1
Copper, Cu 85 - 87 %85 - 87 %
Iron, Fe <= 0.2 %<= 0.2 %
Lead, Pb <= 0.25 %<= 0.25 %not added intentionally; may be specified lower if required
Nickel, Ni <= 1.0 %<= 1.0 %includes Co content
Other, total <= 0.5 %<= 0.5 %
Phosphorus, P <= 0.05 %<= 0.05 %
Selenium, Se 0.8 - 1.1 %0.8 - 1.1 %
Silicon, Si <= 0.005 %<= 0.005 %
Sulfur, S <= 0.08 %<= 0.08 %
Tin, Sn 5.0 - 6.0 %5.0 - 6.0 %
Zinc, Zn 4.0 - 6.0 %4.0 - 6.0 %
 
Descriptive Properties
BrazingGood
Casting Fluidity25 cm at 100F (56C) superheatRagone Test
DrossingLow
SolderingExcellent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 413.0-F Die Casting Alloy
EnviroBrass® (SeBiLOY®) I Lead-Free Casting Alloy, UNS C89510
Aluminum C355.0-T6, Sand Cast
Aluminum A535.0-F or Aluminum 535.0-T5, Cast
Aluminum A356.0-T6, Sand Cast

NSEBIL901 / 147812

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.