MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Haynes 230® alloy, plate, 1000 hours exposure at 760°C (1400°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Excellent high-temperature strength, outstanding resistance to oxidizing environments up to 1149°C, premier resistance to nitriding environments, and excellent long-term thermal stability. Applications include combustion cans, transition ducts, flameholders, thermocouple sheaths and other gas turbine components; used for catalyst grid supports in ammonia burners, high-strength thermocouple protection tubes, high-temperature heat exchangers, ducts, high-temperature bellows; furnace retorts, chains and fixtures, burner flame shrouds, recuperator internals, dampers, nitriding furnace internals, heat-treating baskets, grates, trays, sparger tubes, and cyclone internals.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N06230, AMS 5878, AMS 5891, DIN 17742 No.2.4733
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.97 g/cc0.324 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 885 MPa128000 psi
Tensile Strength, Yield 405 MPa
@Strain 0.2 %
58700 psi
@Strain 0.2 %
Elongation at Break 33 %33 %in 50.8 mm
Modulus of Elasticity 211 GPa30600 ksiRT
 150 GPa
@Temperature 1000 °C
21800 ksi
@Temperature 1830 °F
 157 GPa
@Temperature 900 °C
22800 ksi
@Temperature 1650 °F
 164 GPa
@Temperature 800 °C
23800 ksi
@Temperature 1470 °F
 171 GPa
@Temperature 700 °C
24800 ksi
@Temperature 1290 °F
 177 GPa
@Temperature 600 °C
25700 ksi
@Temperature 1110 °F
 184 GPa
@Temperature 500 °C
26700 ksi
@Temperature 932 °F
 190 GPa
@Temperature 400 °C
27600 ksi
@Temperature 752 °F
 196 GPa
@Temperature 300 °C
28400 ksi
@Temperature 572 °F
 202 GPa
@Temperature 200 °C
29300 ksi
@Temperature 392 °F
 207 GPa
@Temperature 100 °C
30000 ksi
@Temperature 212 °F
Charpy Impact 24.0 J17.7 ft-lb
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000125 ohm-cm0.000125 ohm-cmRT
 0.000125 ohm-cm
@Temperature 1000 °C
0.000125 ohm-cm
@Temperature 1830 °F
 0.0001258 ohm-cm
@Temperature 100 °C
0.0001258 ohm-cm
@Temperature 212 °F
 0.0001265 ohm-cm
@Temperature 200 °C
0.0001265 ohm-cm
@Temperature 392 °F
 0.0001271 ohm-cm
@Temperature 900 °C
0.0001271 ohm-cm
@Temperature 1650 °F
 0.0001273 ohm-cm
@Temperature 300 °C
0.0001273 ohm-cm
@Temperature 572 °F
 0.0001284 ohm-cm
@Temperature 400 °C
0.0001284 ohm-cm
@Temperature 752 °F
 0.0001291 ohm-cm
@Temperature 800 °C
0.0001291 ohm-cm
@Temperature 1470 °F
 0.0001302 ohm-cm
@Temperature 500 °C
0.0001302 ohm-cm
@Temperature 932 °F
 0.0001307 ohm-cm
@Temperature 700 °C
0.0001307 ohm-cm
@Temperature 1290 °F
 0.0001312 ohm-cm
@Temperature 600 °C
0.0001312 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.7 µm/m-°C
@Temperature 25.0 - 100 °C
7.06 µin/in-°F
@Temperature 77.0 - 212 °F
 13.0 µm/m-°C
@Temperature 25.0 - 200 °C
7.22 µin/in-°F
@Temperature 77.0 - 392 °F
 13.3 µm/m-°C
@Temperature 25.0 - 300 °C
7.39 µin/in-°F
@Temperature 77.0 - 572 °F
 13.7 µm/m-°C
@Temperature 25.0 - 400 °C
7.61 µin/in-°F
@Temperature 77.0 - 752 °F
 14.0 µm/m-°C
@Temperature 25.0 - 500 °C
7.78 µin/in-°F
@Temperature 77.0 - 932 °F
 14.4 µm/m-°C
@Temperature 25.0 - 600 °C
8.00 µin/in-°F
@Temperature 77.0 - 1110 °F
 14.8 µm/m-°C
@Temperature 25.0 - 700 °C
8.22 µin/in-°F
@Temperature 77.0 - 1290 °F
 15.2 µm/m-°C
@Temperature 25.0 - 800 °C
8.44 µin/in-°F
@Temperature 77.0 - 1470 °F
 15.7 µm/m-°C
@Temperature 25.0 - 900 °C
8.72 µin/in-°F
@Temperature 77.0 - 1650 °F
 16.1 µm/m-°C
@Temperature 25.0 - 1000 °C
8.94 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.397 J/g-°C0.0949 BTU/lb-°FRT
 0.419 J/g-°C
@Temperature 100 °C
0.100 BTU/lb-°F
@Temperature 212 °F
 0.435 J/g-°C
@Temperature 200 °C
0.104 BTU/lb-°F
@Temperature 392 °F
 0.448 J/g-°C
@Temperature 300 °C
0.107 BTU/lb-°F
@Temperature 572 °F
 0.465 J/g-°C
@Temperature 400 °C
0.111 BTU/lb-°F
@Temperature 752 °F
 0.473 J/g-°C
@Temperature 500 °C
0.113 BTU/lb-°F
@Temperature 932 °F
 0.486 J/g-°C
@Temperature 600 °C
0.116 BTU/lb-°F
@Temperature 1110 °F
 0.574 J/g-°C
@Temperature 700 °C
0.137 BTU/lb-°F
@Temperature 1290 °F
 0.595 J/g-°C
@Temperature 800 °C
0.142 BTU/lb-°F
@Temperature 1470 °F
 0.609 J/g-°C
@Temperature 900 °C
0.146 BTU/lb-°F
@Temperature 1650 °F
 0.617 J/g-°C
@Temperature 1000 °C
0.147 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 8.90 W/m-K61.8 BTU-in/hr-ft²-°FRT
 10.4 W/m-K
@Temperature 100 °C
72.2 BTU-in/hr-ft²-°F
@Temperature 212 °F
 12.4 W/m-K
@Temperature 200 °C
86.1 BTU-in/hr-ft²-°F
@Temperature 392 °F
 14.4 W/m-K
@Temperature 300 °C
99.9 BTU-in/hr-ft²-°F
@Temperature 572 °F
 16.4 W/m-K
@Temperature 400 °C
114 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.4 W/m-K
@Temperature 500 °C
128 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.4 W/m-K
@Temperature 600 °C
142 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.4 W/m-K
@Temperature 700 °C
155 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.4 W/m-K
@Temperature 800 °C
169 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 26.4 W/m-K
@Temperature 900 °C
183 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 28.4 W/m-K
@Temperature 1000 °C
197 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1301 - 1371 °C2374 - 2500 °F
Solidus 1301 °C2374 °F
Liquidus 1371 °C2500 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.30 %0.30 %
Boron, B <= 0.015 %<= 0.015 %
Carbon, C 0.10 %0.10 %
Chromium, Cr 22 %22 %
Cobalt, Co <= 5.0 %<= 5.0 %
Iron, Fe <= 3.0 %<= 3.0 %
Lanthanum, La 0.020 %0.020 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo 2.0 %2.0 %
Nickel, Ni 57 %57 %
Silicon, Si 0.40 %0.40 %
Tungsten, W 14 %14 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tungsten, W
Overview of materials for Copper Alloy
Materion Beryllium Nickel Strip - Alloy 360 Annealed
Haynes Hastelloy® S alloy, flat products
Haynes 230® alloy plate

NH23BE / 16476

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.