MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ovako S355J2 EN10025-2:2004 Steel, +AR
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: S355J2 is a structural carbon-manganese steel suitable for e.g. mechanical engineering applications. Below, a number of closely related variants are presented.
520 M is M-steel variant of S355J2 is as rolled or normalize rolled contrition. 550M is drawn or peeled version of S355

Information provided by Ovako

Key Words: ASt 52, A52 FP, Q420q-D, 1501 Gr.224-460, A52 RBII
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 140 - 190
@Thickness <=16.0 mm
 140 - 190
@Thickness 16.0 - 40.0 mm
 140 - 190
@Thickness 40.0 - 63.0 mm
 140 - 190
@Thickness 63.0 - 80.0 mm
 140 - 190
@Thickness 80.0 - 100 mm
Tensile Strength 470 - 630 MPa
@Thickness <=16.0 mm
 470 - 630 MPa
@Thickness 16.0 - 40.0 mm
 470 - 630 MPa
@Thickness 40.0 - 63.0 mm
 470 - 630 MPa
@Thickness 63.0 - 80.0 mm
 470 - 630 MPa
@Thickness 80.0 - 100 mm
Tensile Strength, Yield >= 315 MPa
@Thickness 80.0 - 100 mm
Rel
 >= 325 MPa
@Thickness 63.0 - 80.0 mm
Rel
 >= 335 MPa
@Thickness 40.0 - 63.0 mm
Rel
 >= 345 MPa
@Thickness 16.0 - 40.0 mm
Rel
 >= 355 MPa
@Thickness <=16.0 mm
Rel
Elongation at Break 20 %
@Thickness 63.0 - 80.0 mm
 20 %
@Thickness 80.0 - 100 mm
 21 %
@Thickness 40.0 - 63.0 mm
 22 %
@Thickness <=16.0 mm
 22 %
@Thickness 16.0 - 40.0 mm
Modulus of Elasticity 210 GPa
Poissons Ratio 0.30
Shear Modulus 80.0 GPa
Impact Test 27.0 J
@Thickness <=16.0 mm,
Temperature -20.0 °C
 27.0 J
@Thickness 16.0 - 40.0 mm,
Temperature -20.0 °C
 27.0 J
@Thickness 40.0 - 63.0 mm,
Temperature -20.0 °C
 27.0 J
@Thickness 63.0 - 80.0 mm,
Temperature -20.0 °C
 27.0 J
@Thickness 80.0 - 100 mm,
Temperature -20.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
Thermal Conductivity 40.0 - 45.0 W/m-KAmbient temperature
Transformation Temperature 400 °CMS
 720 °CAC1
 815 °CAC3
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.24 %
Copper, Cu <= 0.55 %
Iron, Fe >= 97.01 %As Balance
Manganese, Mn <= 1.6 %
Phosphorus, P <= 0.025 %
Silicon, Si <= 0.55 %
Sulfur, S <= 0.025 %
 
Descriptive Properties
WeldabilityCEV 0.52max
 Pcm 0.35max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ovako S355JR EN10025-2:2004 Steel
Ovako S355J2 SB9813 Steel, +AR
ASTM A656 Steel, Grade 7
EN 1.0577 High Manganese, Structural, Hot Rolled, Quality Steel
Ovako S355JR Steel, +AR

NOVAKO420 / 234719

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.