MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
AISI 1006 Steel, CQ, DQ, and DQSK sheet, 1.6-5.8 (0.06-0.23 in) mm thick
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: The composition listed is for standard grade for wire and rod.

Applications: Soft, very ductile, used in applications which require severe bending and welding such as panels for automobiles or appliances. Also used in magnet core applications.

Key Words: UNS G10060, ASME 5041, ASTM A635M, ASTM A830M, FED QQ-W-463, MIL SPEC MIL-S-11310 (CS1006), SAE J403, SAE J412, SAE J416, AISI1006
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.872 g/ccComposition 0.06% C, 0.38% Mn, 0.01% Si, annealed at 925°C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 305 - 360 MPa
Tensile Strength, Yield 180 - 240 MPa
Elongation at Break 32 - 48 %in 50 mm.
Modulus of Elasticity 206 GPa
Bulk Modulus 163 GPaEstimated from elastic modulus
Poissons Ratio 0.29Typical for steel
Machinability 50 %Based on AISI 1212 steel = 100%. Group I bar, rod, and wire products machinability can be improved by cold drawing.
Shear Modulus 80.0 GPaEstimated from elastic modulus
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000174 ohm-cmTypical for 1000 series steels
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.6 µm/m-°C
@Temperature 0.000 - 100 °C
 13.1 µm/m-°C
@Temperature 0.000 - 200 °C
 13.5 µm/m-°C
@Temperature 0.000 - 300 °C
 13.7 µm/m-°C
@Temperature 0.000 - 400 °C
 13.7 µm/m-°C
@Temperature 0.000 - 1000 °C
 14.2 µm/m-°C
@Temperature 0.000 - 500 °C
 14.6 µm/m-°C
@Temperature 0.000 - 600 °C
 14.9 µm/m-°C
@Temperature 0.000 - 700 °C
 16.6 µm/m-°C
@Temperature 0.000 - 800 °C
Specific Heat Capacity 0.481 J/g-°C
@Temperature >=100 °C
 0.519 J/g-°C
@Temperature 150 - 200 °C
 0.536 J/g-°C
@Temperature 200 - 250 °C
 0.553 J/g-°C
@Temperature 250 - 300 °C
 0.595 J/g-°C
@Temperature 350 - 400 °C
 0.662 J/g-°C
@Temperature 450 - 500 °C
 0.754 J/g-°C
@Temperature 550 - 600 °C
 0.846 J/g-°C
@Temperature 850 - 900 °C
 0.867 J/g-°C
@Temperature 650 - 700 °C
 1.105 J/g-°C
@Temperature 700 - 750 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.080 %
Iron, Fe 99.43 - 99.75 %As remainder
Manganese, Mn 0.25 - 0.40 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1008 Steel, CQ, DQ, and DQSK sheet, 1.6-5.8 mm thick
AISI 1006 Steel, cold drawn
AISI 1006 Steel, cold drawn bar, 19-32 mm (0.75-1.25 in) round
AISI 1006 Steel, hot rolled bar, 19-32 mm (0.75-1.25 in) round
AISI 1010 Steel, CQ sheet,1.6-5.8 mm round or thickness

M1006D / 6777

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.