MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 10844 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 10844 is an 80 durometer black colored fluorinated hydrocarbon elastomer, it is formulated with FDA sanctioned materials. It exhibits good resistance to heat, petroleum based oils, aliphatic and aromatic fuels

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 820 A1-10 B37 B38 EF31 EO78 4 HK 820 A1-11 B38 EF31 EO78; 6 HK 820 A1-10 A1-11 EF31 EO38
CFR 21 177.2600

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.84 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 82
 73
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 76
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 79
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 80
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 81
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 82
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 86
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
Tensile Strength 2207 psi
 1933.3 psi
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 1940 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1988.5 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 2103.3 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 2127.5 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 2390.2 psi
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 166 %
 153.4 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 160.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 181.3 %
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 189.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 200 %
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 1602.8 %
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
50% Modulus 577 psi
100% Modulus 1266 psi
Tear Strength 12.6 pliDie C; Method D 624
 200.9 pliDie B; Method D 624
Compression Set 13 %
@Treatment Temp. 175 °C,
Time 79200 sec
Plied
 16.7 %
@Treatment Temp. 200 °C,
Time 79200 sec
Plied
 19.2 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -12.0 °F
Shrinkage 1.6 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 3.5 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 3.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 10.8 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 17.6 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBlack
TR-10 Temperature-19°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL136 / 318346

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.