MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Pressure Seal 10844 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 10844 is an 80 durometer black colored fluorinated hydrocarbon elastomer, it is formulated with FDA sanctioned materials. It exhibits good resistance to heat, petroleum based oils, aliphatic and aromatic fuels

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 820 A1-10 B37 B38 EF31 EO78 4 HK 820 A1-11 B38 EF31 EO78; 6 HK 820 A1-10 A1-11 EF31 EO38
CFR 21 177.2600

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.84 g/cc1.84 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8282
 73
@Treatment Temp. 200 °C,
Time 252000 sec
73
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 76
@Treatment Temp. 200 °C,
Time 252000 sec
76
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 79
@Treatment Temp. 100 °C,
Time 252000 sec
79
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 80
@Treatment Temp. 150 °C,
Time 252000 sec
80
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 81
@Treatment Temp. 23.0 °C,
Time 252000 sec
81
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 82
@Treatment Temp. 250 °C,
Time 252000 sec
82
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 86
@Treatment Temp. 275 °C,
Time 252000 sec
86
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
Tensile Strength 15.22 MPa2207 psi
 13.330 MPa
@Treatment Temp. 275 °C,
Time 252000 sec
1933.3 psi
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 13.4 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1940 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 13.710 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
1988.5 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 14.502 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
2103.3 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 14.669 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
2127.5 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 16.480 MPa
@Treatment Temp. 250 °C,
Time 252000 sec
2390.2 psi
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
Elongation, Ultimate 166 %166 %
 153.4 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
153.4 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 160.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
160.7 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 181.3 %
@Treatment Temp. 275 °C,
Time 252000 sec
181.3 %
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 189.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
189.9 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 200 %
@Treatment Temp. 200 °C,
Time 252000 sec
200 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 1602.8 %
@Treatment Temp. 250 °C,
Time 252000 sec
1602.8 %
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
50% Modulus 3.98 MPa3.98 MPa
100% Modulus 8.729 MPa1266 psi
Tear Strength 2.21 kN/m12.6 pliDie C; Method D 624
 35.22 kN/m200.9 pliDie B; Method D 624
Compression Set  13 %
@Treatment Temp. 175 °C,
Time 79200 sec
13 %
@Treatment Temp. 347 °F,
Time 22.0 hour
Plied
 16.7 %
@Treatment Temp. 200 °C,
Time 79200 sec
16.7 %
@Treatment Temp. 392 °F,
Time 22.0 hour
Plied
 19.2 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
19.2 %
@Treatment Temp. 73.4 °F,
Time 22.0 hour
Plied
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -24.4 °C-12.0 °F
Shrinkage  1.6 %
@Treatment Temp. 150 °C,
Time 252000 sec
1.6 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 3.5 %
@Treatment Temp. 100 °C,
Time 252000 sec
3.5 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, Distilled water aged
 3.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
3.6 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel C
 10.8 %
@Treatment Temp. 200 °C,
Time 252000 sec
10.8 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Service Fluid 100
 17.6 %
@Treatment Temp. 200 °C,
Time 252000 sec
17.6 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBlack
TR-10 Temperature-19°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL136 / 318346

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.