MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
LyondellBasell Moplen CA012/1 Polypropylene, Impact Modified; Molded/Extruded  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Impact Modified; Molded/Extruded

Material Notes: Moplen CA012/1 is a nucleated polypropylene impact copolymer used in injection and compression molding caps & closures applications. Moplen CA012/1 is a proprietary grade and can only be used by processors with the appropriate Global Closure Systems (GCS) license. Applications: Caps & Closures

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccISO 1183-1
Melt Flow 6.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133-1
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 64.0 MPaISO 2039-1
Tensile Strength, Yield 30.0 MPaISO 527-1,-2
Elongation at Break >= 50 %ISO 527-1,-2
Elongation at Yield 7.0 %ISO 527-1,-2
Tensile Modulus 1500 MPaISO 527-1,-2
Charpy Impact, Notched 3.50 kJ/m²
@Temperature -20.0 °C
Type 1, Edgewise, Notch A; ISO 179
 4.50 kJ/m²
@Temperature 0.000 °C
Type 1, Edgewise, Notch A; ISO 179
 8.50 kJ/m²
@Temperature 23.0 °C
Type 1, Edgewise, Notch A; ISO 179
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 100 °Cunannealed; ISO 75B-1,-2
Vicat Softening Point 151 °CA50; ISO 306
 
Descriptive Properties
Ball Indentation Hardness (MPa)H 358/30
Processing MethodInjection Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Hostacom PP HH42L 356015 Polypropylene
LyondellBasell Hostalen PP H2142 12 Polypropylene Copolymer
LyondellBasell Moplen 2000HEXP Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Hostalen PP H1850 Polypropylene Copolymer
LyondellBasell Hostalen PP H1022 Polypropylene Copolymer

PEQT8890 / 220524

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.