MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AGC AFLAS® 150E TFE/P Fluoroelastomers
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: AFLAS® Fluoroelastomers are copolymers of tetrafluoroethylene and propylene. This combination gives AFLAS® Fluoroelastomers unique properties over conventional FKM-type fluoroelastomers in demanding applications found in the oil & gas, chemical process, wire & cable, industrial equipment, food handling, pharmaceutical, heavy duty diesel and automotive industries. AFLAS Fluoroelastomers display outstanding resistance to heat, acids & bases, many solvents, ozone, and steam. Classified by ASTM D 1418-01 as FEPM.

Material Features:

    Excellent base and amine resistance unmatched by FKM-type fluoroelastomers
  • Extremely high electrical resistivity, compared with other elastomers
  • High heat resistance compared to FKMs
  • Outstanding steam resistance
  • Low viscosity
  • Excellent elongation
End User Benefits:
    Excellent processing for extrusion
  • Compression / transfer molding are also applicable
Typical Applications:
    Wire insulator
  • Cable jacket
  • Hoses, tubes
  • Sheets

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Mooney Viscosity 45
@Temperature 121 °C
[kN/m], (ML1+10)
 60
@Temperature 100 °C
[kN/m], (ML1+10)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 13.0 MPa
 11.83 MPa
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
Hot Water Resistance
 11.96 MPa
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
Steam Resistance
 13.65 MPa
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
50% NaOH aq Resistance
 13.65 MPa
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
28% Aq Ammonia Resistance
 15.21 MPa
@Treatment Temp. 200 °C,
Time 2.59e+6 sec
Heat Resistance
Elongation at Break 360 %
 291.6 %
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
28% Aq Ammonia Resistance
 302.4 %
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
50% NaOH aq Resistance
 370.8 %
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
Hot Water Resistance
 370.8 %
@Treatment Temp. 200 °C,
Time 2.59e+6 sec
Heat Resistance
 399.6 %
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
Steam Resistance
Tensile Modulus 0.160 MPaG' Storage Modulus (nominal) of Raw Gum
100% Modulus 0.00500 GPa
@Strain 100 %
Compression Set 32 %
@Temperature 200 °C,
Time 252000 sec
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -40.0 °CBrittle Point
 3.00 °CTR-10
Glass Transition Temp, Tg -3.00 °C
 
Processing PropertiesOriginal ValueComments
Cure Time 0.900 min
@Temperature 177 °C
10% cure, tc10, 100CPM, 3° Strain, 12 minutes
 2.30 min
@Temperature 177 °C
50% cure, tc50, 100CPM, 3° Strain, 12 minutes
 4.00 hour
@Temperature 200 °C
Post cure
 7.10 min
@Temperature 177 °C
90% cure, 100CPM, 3° Strain, 12 minutes
 20.0 min
@Temperature 170 °C
Press
 
Component Elements PropertiesOriginal ValueComments
Fluorine, F 57 %
 
Descriptive Properties
Cure Data2.5 dNmMin S'
 27.9 dNmMax S'
Volume Change0%50% NaOH Resistance 70°C for 720 hours
Volume Change (%)11Steam Resistance 180°C for 720 hours
 228% Aqueous Ammonia Resistance 70°C for 720 hours
 20Hot water Resistance 180°C for 720 hours

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AGC AFLAS® PM-1100 TFE/P Perfluoroelastomer
AGC AFLAS® 300S TFE/P Latex
AGC AFLAS® 200P TFE/P Fluoroelastomers
AGC AFLAS® 150P TFE/P Fluoroelastomers
AGC AFLAS® 150L TFE/P Fluoroelastomers

PAGCX008 / 191117

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.