MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Dow INTEGRAL™ 917 Monolayer Bonding Film  (discontinued **)
Categories: Polymer; Film; Thermoset

Material Notes: INTEGRAL 917 Adhesive Film is a single layer adhesive film for use where a higher flow rate and lower melt point are required. It is useful for bonding heat sensitive materials, or for porous substrates, and can be used to bond fabric to foam, paper to foil, or olefin sheet to non-woven textiles.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Thickness 50.8 microns2.00 mil
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 10.3 MPa1500 psiASTM D882
Film Tensile Strength at Yield, TD 8.27 MPa1200 psiASTM D882
Film Elongation at Break, MD 200 %200 %ASTM D882
Film Elongation at Break, TD 400 %400 %ASTM D882
Secant Modulus, MD 0.131 GPa19.0 ksi2% Secant; ASTM D882
Secant Modulus, TD 0.138 GPa20.0 ksi2% Secant; ASTM D882
Elmendorf Tear Strength, MD 5.51 g/micron140 g/milASTM D882
Elmendorf Tear Strength, TD 3.74 g/micron95.0 g/milASTM D882
Film Tensile Strength at Break, MD 25.5 MPa3700 psiASTM D882
Film Tensile Strength at Break, TD 16.5 MPa2400 psiASTM D882

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Rogers Arlon CuClad 6250 Bonding Film
Rogers Arlon CLTE-P Pre-Preg Bonding Layer
Morgan Advanced Ceramics Kaowool® Paper 3000 Thermal Ceramic
Morgan Advanced Ceramics Kaowool M Organic RCF Vacuum Formed Thermal Ceramic
Honeywell UltRx 400 CTFE Homopolymer, Barrier Film

PDOW1051 / 30255

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.