MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hexcel® HexPly® M12 135°C Curing Epoxy Matrix, 37%/7781 Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy Cure Resin

Material Notes:

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.24 g/cc0.0448 lb/in³Resin Density
 2.60 g/cc0.0939 lb/in³Fiber Density
Filler Content 50.0 %50.0 %Fiber Volume
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 415 MPa60200 psi90º, RT, Dry; EN2561
 510 MPa74000 psiRT; Dry; EN2561
 270 MPa
@Temperature 75.0 °C
39200 psi
@Temperature 167 °F
Wet; EN2561
 270 MPa
@Temperature 100 °C
39200 psi
@Temperature 212 °F
Wet; EN2561
 270 MPa
@Temperature 75.0 °C
39200 psi
@Temperature 167 °F
90º, Wet; EN2561
 300 MPa
@Temperature 100 °C
43500 psi
@Temperature 212 °F
90º, Wet; EN2561
Tensile Modulus 26.0 GPa3770 ksi90º, RT, Dry; EN2561
 29.0 GPa4210 ksiRT; Dry; EN2561
 25.0 GPa
@Temperature 100 °C
3630 ksi
@Temperature 212 °F
90º, Wet; EN2561
 26.0 GPa
@Temperature 75.0 °C
3770 ksi
@Temperature 167 °F
90º, Wet; EN2561
 27.0 GPa
@Temperature 100 °C
3920 ksi
@Temperature 212 °F
Wet; EN2561
 28.0 GPa
@Temperature 75.0 °C
4060 ksi
@Temperature 167 °F
Wet; EN2561
Compressive Yield Strength 460 MPa66700 psi90º, RT, Dry; DIN65380
 500 MPa72500 psiRT; Dry; DIN65380
 320 MPa
@Temperature 100 °C
46400 psi
@Temperature 212 °F
90º, Wet; DIN65380
 360 MPa
@Temperature 100 °C
52200 psi
@Temperature 212 °F
Wet; DIN65380
 380 MPa
@Temperature 75.0 °C
55100 psi
@Temperature 167 °F
Wet; DIN65380
 400 MPa
@Temperature 75.0 °C
58000 psi
@Temperature 167 °F
90º, Wet; DIN65380
Compressive Modulus 27.0 GPa3920 ksi90º, RT, Dry; DIN65380
 30.0 GPa4350 ksiRT; Dry; DIN65380
 25.0 GPa
@Temperature 100 °C
3630 ksi
@Temperature 212 °F
90º, Wet; DIN65380
 26.0 GPa
@Temperature 75.0 °C
3770 ksi
@Temperature 167 °F
Wet; DIN65380
 26.0 GPa
@Temperature 100 °C
3770 ksi
@Temperature 212 °F
Wet; DIN65380
 26.0 GPa
@Temperature 75.0 °C
3770 ksi
@Temperature 167 °F
90º, Wet; DIN65380
Shear Strength 80.0 MPa11600 psiIn-Plane, RT, Dry; EN6031
 83.0 MPa12000 psi0º, ILSS (Short Beam), RT, Dry; EN2563
 37.0 MPa
@Temperature 100 °C
5370 psi
@Temperature 212 °F
0º, ILSS (Short Beam), Wet; EN2563
 43.0 MPa
@Temperature 75.0 °C
6240 psi
@Temperature 167 °F
0º, ILSS (Short Beam), Wet; EN2563
 70.0 MPa
@Temperature 100 °C
10200 psi
@Temperature 212 °F
In-Plane, Wet; EN6031
 75.0 MPa
@Temperature 75.0 °C
10900 psi
@Temperature 167 °F
In-Plane, Wet; EN6031
 
Processing PropertiesMetricEnglishComments
Shelf Life 14.0 Month
@Temperature -18.0 °C
14.0 Month
@Temperature -0.400 °F
 
Descriptive Properties
Cured Thickness per Ply (cm)0.23

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hexcel® HexPly® M12 135°C Curing Epoxy Matrix, TVR380/26% Fiber
Solvay CYCOM® 919 Epoxy Prepreg System with Woven E Glass Fiber 7781
Park Aerospace Nelcote® E-718 Epoxy Prepreg, 7781 E-Glass Reinforced
Solvay CYCOM® 381 Epoxy Prepreg with CYCOM 7781 OST E-glass Fabric and 300FAW Epoxy
Overview of materials for High Carbon Steel

PHEXC157 / 98627

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.