Physical Properties | Metric | English | Comments |
---|
Density | 0.928 g/cc | 0.0335 lb/in³ |
Viscosity | 203 cP @Shear Rate 206 1/s, Temperature 200 °C | 203 cP @Shear Rate 206 1/s, Temperature 392 °F |
Linear Mold Shrinkage | 0.012 cm/cm | 0.012 in/in |
Linear Mold Shrinkage, Transverse | 0.012 cm/cm | 0.012 in/in |
Melt Flow | 12 g/10 min @Load 2.16 kg, Temperature 230 °C | 12 g/10 min @Load 4.76 lb, Temperature 446 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore D | 38 @Time 15.0 sec | 38 @Time 0.00417 hour |
| 39 @Time 5.00 sec | 39 @Time 0.00139 hour |
| 44 @Time 1.00 sec | 44 @Time 0.000278 hour |
| 38.7 @Treatment Temp. 125 °C, Time 15.0 sec | 38.7 @Treatment Temp. 257 °F, Time 0.00417 hour |
| 39.3 @Treatment Temp. 125 °C, Time 5.00 sec | 39.3 @Treatment Temp. 257 °F, Time 0.00139 hour |
| 39.9 @Treatment Temp. 110 °C, Time 15.0 sec | 39.9 @Treatment Temp. 230 °F, Time 0.00417 hour |
| 40 @Treatment Temp. 110 °C, Time 5.00 sec | 40 @Treatment Temp. 230 °F, Time 0.00139 hour |
| 43.1 @Treatment Temp. 125 °C, Time 1.00 sec | 43.1 @Treatment Temp. 257 °F, Time 0.000278 hour |
| 45.7 @Treatment Temp. 110 °C, Time 1.00 sec | 45.7 @Treatment Temp. 230 °F, Time 0.000278 hour |
Tensile Strength at Break | 13.4 MPa | 1940 psi |
| 14.9 MPa | 2160 psi |
| 12.2 MPa @Treatment Temp. 125 °C, Time 605000 sec | 1770 psi @Treatment Temp. 257 °F, Time 168 hour |
| 13.0 MPa @Treatment Temp. 110 °C, Time 3.629e+6 sec | 1880 psi @Treatment Temp. 230 °F, Time 1008 hour |
| 14.6 MPa @Treatment Temp. 125 °C, Time 605000 sec | 2120 psi @Treatment Temp. 257 °F, Time 168 hour |
| 14.7 MPa @Treatment Temp. 110 °C, Time 3.629e+6 sec | 2130 psi @Treatment Temp. 230 °F, Time 1008 hour |
Tensile Stress at Strain | 6.13 MPa @Strain 100 % | 889 psi @Strain 100 % |
| 7.31 MPa @Strain 100 % | 1060 psi @Strain 100 % |
Elongation at Break | 630 % | 630 % |
| 720 % | 720 % |
| 64.8 % @Treatment Temp. 125 °C, Time 605000 sec | 64.8 % @Treatment Temp. 257 °F, Time 168 hour |
| 523 % @Treatment Temp. 125 °C, Time 605000 sec | 523 % @Treatment Temp. 257 °F, Time 168 hour |
| 567 % @Treatment Temp. 110 °C, Time 3.629e+6 sec | 567 % @Treatment Temp. 230 °F, Time 1008 hour |
| 694 % @Treatment Temp. 110 °C, Time 3.629e+6 sec | 694 % @Treatment Temp. 230 °F, Time 1008 hour |
Tear Strength | 59.6 kN/m | 340 pli |
| 66.6 kN/m | 380 pli |
Compression Set | 37 % @Temperature 22.8 °C, Time 79200 sec | 37 % @Temperature 73.0 °F, Time 22.0 hour |
| 56 % @Temperature 70.0 °C, Time 79200 sec | 56 % @Temperature 158 °F, Time 22.0 hour |
| 68 % @Temperature 90.0 °C, Time 252000 sec | 68 % @Temperature 194 °F, Time 70.0 hour |
| 100 % @Temperature 125 °C, Time 252000 sec | 100 % @Temperature 257 °F, Time 70.0 hour |
|
Processing Properties | Metric | English | Comments |
---|
Rear Barrel Temperature | 199 - 210 °C | 390 - 410 °F |
Middle Barrel Temperature | 204 - 216 °C | 400 - 420 °F |
Front Barrel Temperature | 210 - 221 °C | 410 - 430 °F |
Nozzle Temperature | 216 - 227 °C | 420 - 440 °F |
Melt Temperature | 216 - 227 °C | 420 - 440 °F |
Mold Temperature | 15.6 - 32.2 °C | 60.0 - 90.0 °F |
Injection Pressure | 1.38 - 5.52 MPa | 200 - 800 psi |
Back Pressure | 0.172 - 0.862 MPa | 25.0 - 125 psi |
Cushion | 0.381 - 2.54 cm | 0.150 - 1.00 in |
Screw Speed | 50 - 120 rpm | 50 - 120 rpm |
|
Descriptive Properties |
---|
Appearance | Black |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.