Kolon ELLAS K-390A Ether Based Thermoplastic Polyurethane
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Elastomer, TPE
;
Polyurethane, TP
;
Thermoplastic Polyurethane, Elastomer, Ether Grade
Material Notes:
Applications
Extrusion: Cable Sheathing, high pressure tube
Injection
Electric Wire
Industry Parts
Information provided by API-Kolon.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.12
g/cc
1.12
g/cc
ASTM D792
Mechanical Properties
Metric
English
Comments
Hardness, Shore A
90
90
ASTM D2240
Tensile Strength
46.1
MPa
6680
psi
ASTM D412
Tensile Stress at Strain
8.83
MPa
@Strain 100 %
1280
psi
@Strain 100 %
ASTM D412
Elongation at Break
500 %
500 %
ASTM D412
Tear Strength
123
kN/m
700
pli
ASTM D624
Processing Properties
Metric
English
Comments
Nozzle Temperature
185
-
195
°C
365
-
383
°F
Injection Molding
Zone 1
155
-
175
°C
311
-
347
°F
Extrusion Molding
160
-
175
°C
320
-
347
°F
Injection Molding
Zone 2
170
-
185
°C
338
-
365
°F
Extrusion Molding
175
-
185
°C
347
-
365
°F
Injection Molding
Zone 3
170
-
190
°C
338
-
374
°F
Extrusion Molding
180
-
190
°C
356
-
374
°F
Injection Molding
Zone 4
180
-
195
°C
356
-
383
°F
Extrusion Molding
Die Temperature
180
-
195
°C
356
-
383
°F
Extrusion Molding
Head Temperature
190
-
200
°C
374
-
392
°F
Extrusion Molding
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Huntsman IROGRAN® A 95 P 5044 DP TPU-Polyether
BASF Elastollan® 1190A Polyether Type Polyurethane Elastomer
C.O.I.M. LARIPUR® LPR2103-90AE PTMG Polyether Polyurethane
Dow PELLETHANE® 2101-85A Polyurethane Elastomer (Ether-Ether Hybrid)
Dow Pellethane® 2103-90AEF Polyurethane Elastomer, Ether Based
PKOKZ984 / 122686
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.