MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Wolf Kunststoff ZEDEX® ZX-750V5T A9T Polymer Alloy
Categories: Polymer; Thermoplastic

Material Notes: Main Characteristics: Hard; Stiff; Tough; High dimensional stability; High fatigue strength; High weather resistance; Good fire behavior; Suitable for vacuum; Good machinability; Contains PTFE; Stress resistant
Applications: Textile Machinery; Compressors; Hinges; Handling; Machine Tools; Automitve Technology

Information provided by Zedex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.44 g/cc0.0520 lb/in³ISO 1183
Water Absorption 0.20 %
@Temperature 23.0 °C
0.20 %
@Temperature 73.4 °F
RMC 93%; DIN EN ISO 62
Moisture Absorption at Equilibrium 0.50 %0.50 %DIN EN ISO 62
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A >= 100>= 100DIN 53505
Hardness, Shore D 8585DIN 53505
Ball Indentation Hardness 110 MPa16000 psiDIN 2039
Tensile Strength at Break 45.0 MPa6530 psiDIN EN ISO 527
Tensile Strength 45.0 MPa6530 psiDIN EN ISO 527
Tensile Strength, Yield 35.8 MPa5190 psiElastic Limit
Tensile Stress at Strain 35.0 MPa
@Strain 1 %,
Time 3.60e+6 sec
5080 psi
@Strain 1 %,
Time 1000 hour
DIN 53444
Elongation at Break 3.1 %3.1 %DIN EN ISO 527
Elongation at Yield 2.1 %2.1 %Elastic Yield Point
 3.1 %3.1 %Elongation at Maximum Force; DIN EN ISO 527
Tensile Modulus 3.10 GPa450 ksiDIN EN ISO 527
Flexural Strength 68.0 MPa9860 psiDIN EN ISO 178
 68.0 MPa9860 psiDIN EN ISO 178
 103 MPa14900 psiOuter Fiber Stress at 3.5% Outer Fiber Strain; DIN EN ISO 178
Flexural Modulus 3.32 GPa482 ksiDIN EN ISO 178
Flexural Strain at Break 3.1 %3.1 %DIN EN ISO 178
Flexural Strain at Yield 2.2 %2.2 %DIN EN ISO 178
Compressive Strain at Break 9.9 %9.9 %Nominal Compressive Strain at Compressive Strength; DIN EN ISO 604
Compressive Strain at Yield 9.9 %9.9 %Nominal; DIN EN ISO 604
Compressive Yield Strength 95.0 MPa13800 psiElastic Limit
 115 MPa16700 psiDIN EN ISO 604
Compressive Strength 112 MPa16200 psibreak; DIN EN ISO 604
 115 MPa16700 psiDIN EN ISO 604
 48.0 MPa
@Time 3.60e+7 sec
6960 psi
@Time 10000 hour
 86.0 MPa
@Time 360000 sec
12500 psi
@Time 100 hour
 102 MPa
@Time 36.0 sec
14800 psi
@Time 0.0100 hour
 19.0 MPa
@Strain 3.5 %
2760 psi
@Strain 3.5 %
DIN EN ISO 604
Compressive Modulus 4.011 GPa581.7 ksiDIN EN ISO 604
Fatigue Strength 35.0 MPa
@# of Cycles 1.00e+6
5080 psi
@# of Cycles 1.00e+6
1 Hz
K Factor (ISO)  0.40 µm/km
@Temperature 100 °C
0.40 µm/km
@Temperature 212 °F
 0.50 µm/km
@Temperature 200 °C
0.50 µm/km
@Temperature 392 °F
 0.50 µm/km
@Temperature 240 °C
0.50 µm/km
@Temperature 464 °F
 1.5 µm/km
@Temperature 20.0 °C
1.5 µm/km
@Temperature 68.0 °F
Charpy Impact Unnotched NBNBEN ISO 179/1eU
Charpy Impact, Notched 2.47 J/cm²11.8 ft-lb/in²EN ISO 179/1eA
Coefficient of Friction, Dynamic  0.17
@Temperature 20.0 °C
0.17
@Temperature 68.0 °F
Dry Operation
 0.20
@Temperature 100 °C
0.20
@Temperature 212 °F
Dry Operation
Coefficient of Friction, Static 0.19
@Temperature 20.0 °C
0.19
@Temperature 68.0 °F
Dry Operation
Tensile Creep Modulus, 1000 hours 3200 MPa464000 psiAt 1% Deformation; DIN 53444
Limiting Pressure Velocity 0.83333 MPa-m/sec23792 psi-ft/minv = 1m/min
 2.50 MPa-m/sec71400 psi-ft/minv = 200m/min
 2.567 MPa-m/sec73280 psi-ft/minv = 10m/min
 3.90 MPa-m/sec111000 psi-ft/minv = 100m/min
Compression Set 6.0 %6.0 %Elastic Compression Limit
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmIEC 93
Surface Resistance 5.00e+12 ohm5.00e+12 ohmIEC 93
Dielectric Constant 3.1
@Frequency 110 Hz
3.1
@Frequency 110 Hz
IEC 250
Dielectric Strength 21.0 kV/mm533 kV/inIEC 243
Dissipation Factor 0.000800.00080IEC 112
 0.078
@Frequency 110 Hz
0.078
@Frequency 110 Hz
Comparative Tracking Index 42 V42 VIEC 112
 
Thermal PropertiesMetricEnglishComments
CTE, linear  40.0 µm/m-°C
@Temperature <=100 °C
22.2 µin/in-°F
@Temperature <=212 °F
ISO E 830
 47.0 µm/m-°C
@Temperature <=150 °C
26.1 µin/in-°F
@Temperature <=302 °F
ISO E 831
Specific Heat Capacity 1.18 J/g-°C0.282 BTU/lb-°FDSC
Melting Point 390 °C734 °FDSC
Maximum Service Temperature, Air 250 °C482 °FPressed Bushings
 280 °C536 °FContinuous
 320 °C608 °FShort Term (3h)
Deflection Temperature at 1.8 MPa (264 psi) 250 °C482 °FDIN EN ISO 75
Glass Transition Temp, Tg 240 °C464 °FDSC
Flammability, UL94 V-0V-0
Oxygen Index 52 %52 %DIN EN ISO 4589
 
Descriptive Properties
Alignment Adjustment4Nominal Scale: 1, low; 10, high
Chemical Sterilization10Nominal Scale: 1, low; 10, high
ColorOchre
Creep Resistance3Nominal Scale: 1, low; 10, high
Dimensional Stability with Thermal Expansion9Nominal Scale: 1, low; 10, high
Free from SiliconApplicable
Gamma-rays Radiation Sterilization7Nominal Scale: 1, low; 10, high
Machined PartsApplicable
Moist Heat Sterilization6Nominal Scale: 1, low; 10, high
Resistance Against dust, Dirt, Abrasive Substances5Nominal Scale: 1, low; 10, high
Resistance Against Hot Water120
Resistance to Chemicals5Nominal Scale: 1, low; 10, high
Resistant Against DisinfectantApplicable
Rods up to Øe (de)Applicable
ROHS/WEEEApplicable
Sheets up to Maximum ThicknessApplicable
Sliding Velocity350
Suitable for Outdoor Use9Nominal Scale: 1, low; 10, high
Suitable for VacuumApplicable
UV Rays Resistance9Nominal Scale: 1, low; 10, high

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Epoxy Encapsulant, Unreinforced
Overview of materials for Epoxy, Electrically Conductive
Overview of materials for Polyimide
Overview of materials for Silicone, Molded, Glass Fiber Filled
Wolf Kunststoff ZEDEX® ZX-750V5KF 055 Fiber Reinforced Polymer Alloy

PZEDEX18 / 122133

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.