MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
AISI 1008 Steel, hot rolled bar, 19-32 mm (0.75-1.25 in) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Usually produced as rimmed, capped, semikilled, and fully killed, Rimmed have exceptional cold formability. Weldability (spot, projection, butt, and fusion) and brazeability are excellent. Applications include extruded, cold headed, cold upset, and cold pressed parts and forms.

Key Words: UNS G10080, JIS G3141(96) SPCC, ASTM A29, ASTM A108, ASTM A510, ASTM A512, ASTM A513, ASTM A519, ASTM A545, ASTM A575, ASTM A576, ASTM A619, ASTM A620, ASTM A621, ASTM A622, ASTM A635, FED QQ-S-637 (C1008), FED QQ-S-698 (C1008), FED QQ-W-461, MIL SPEC MIL R-8814, MIL SPEC MIL S-11310 (CS1008,1008), SAE J1397, SAE J403, SAE J412, SAE J414, DIN 1.0204, UNI CB10 FU, AISI1008
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.872 g/ccComposition 0.06% C, 0.38% Mn, 0.01% Si, annealed at 925°C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 86
Hardness, Knoop 103Converted from Brinell
Hardness, Rockwell B 49Converted from Brinell
Hardness, Vickers 88Converted from Brinell
Tensile Strength, Ultimate 305 MPa
Tensile Strength, Yield 170 MPa
Elongation at Break 30 %in 50 mm
Reduction of Area 55 %
Modulus of Elasticity 200 GPa
Bulk Modulus 160 GPaTypical for steel
Poissons Ratio 0.29Typical For Steel
Machinability 55 %Based on AISI 1212 steel = 100%. Group I bar, rod, and wire products machinability can be improved by cold drawing.
Shear Modulus 80.0 GPaTypical for steel
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000142 ohm-cm
@Temperature 20.0 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0000190 ohm-cm
@Temperature 100 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0000263 ohm-cm
@Temperature 200 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0000458 ohm-cm
@Temperature 400 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0000734 ohm-cm
@Temperature 600 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0000905 ohm-cm
@Temperature 700 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0001081 ohm-cm
@Temperature 800 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.000113 ohm-cm
@Temperature 900 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0001193 ohm-cm
@Temperature 1100 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 0.0001216 ohm-cm
@Temperature 1200 °C
annealed specimen, Composition 0.08% C, 0.31% Mn.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.6 µm/m-°C
@Temperature 0.000 - 100 °C
 13.1 µm/m-°C
@Temperature 0.000 - 200 °C
 13.5 µm/m-°C
@Temperature 0.000 - 300 °C
 13.7 µm/m-°C
@Temperature 0.000 - 400 °C
 13.7 µm/m-°C
@Temperature 0.000 - 1000 °C
 14.2 µm/m-°C
@Temperature 0.000 - 500 °C
 14.6 µm/m-°C
@Temperature 0.000 - 600 °C
 14.9 µm/m-°C
@Temperature 0.000 - 700 °C
 16.6 µm/m-°C
@Temperature 0.000 - 800 °C
Specific Heat Capacity 0.481 J/g-°C
@Temperature >=100 °C
annealed
 0.519 J/g-°C
@Temperature 150 - 200 °C
 0.536 J/g-°C
@Temperature 200 - 250 °C
 0.553 J/g-°C
@Temperature 250 - 300 °C
 0.595 J/g-°C
@Temperature 350 - 400 °C
 0.662 J/g-°C
@Temperature 450 - 500 °C
 0.754 J/g-°C
@Temperature 550 - 600 °C
 0.846 J/g-°C
@Temperature 850 - 900 °C
 0.867 J/g-°C
@Temperature 650 - 700 °C
 1.105 J/g-°C
@Temperature 700 - 750 °C
Thermal Conductivity 27.3 W/m-K
@Temperature 1000 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 28.4 W/m-K
@Temperature 800 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 36.3 W/m-K
@Temperature 600 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 45.2 W/m-K
@Temperature 400 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 54.7 W/m-K
@Temperature 200 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 60.2 W/m-K
@Temperature 100 °C
Composition of 0.06% Carbon, 0.4% Manganese.
 65.2 W/m-K
@Temperature 0.000 °C
Composition of 0.06% Carbon, 0.4% Manganese.
Melting Point 1426 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.10 %
Iron, Fe 99.31 - 99.7 %As remainder
Manganese, Mn 0.30 - 0.50 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1008 Steel, cold drawn bar, 19-32 mm (0.75-1.25 in) round
AISI 1008 Steel, CQ, DQ, and DQSK sheet, 1.6-5.8 mm thick
AISI 1010 Steel, hot rolled bar, 19-32 mm (0.75-1.25 in) round or thickness
AISI 1010 Steel, cold drawn
Eagle Brass 1008 Low Carbon Steel, Annealed

M1008B / 6778

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.