MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Crastin® CE2055 NC010 Polybutylene Terephthalate (PBT)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Unreinforced Low Viscosity Polybutylene Terephthalate

Crastin CE2055 NC010 is an unreinforced low viscosity polybutylene terephthalate resin for injection molding.

Former DuPont product acquired by Celanese in 2022.

Key Words: PBT
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.31 g/ccISO 1183
Water Absorption 0.40 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.017 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.017 cm/cmISO 294-4, 2577
Melt Flow 43 g/10 min
@Load 2.16 kg,
Temperature 250 °C
cm³/10min Volumetric; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 60.0 MPaISO 527-1/-2
Elongation at Break 13 %Nominal; ISO 527-1/-2
Elongation at Yield 10 %ISO 527-1/-2
Tensile Modulus 2600 MPaISO 527-1/-2
Flexural Strength 82.0 MPaISO 178
Poissons Ratio 0.38
Izod Impact, Notched (ISO) 3.90 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Charpy Impact, Notched 3.50 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 150 °CISO 75-1/-2
 183 °CAnnealed; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °CISO 75-1/-2
 58.0 °CAnnealed; ISO 75-1/-2
Vicat Softening Point 175 °C50°C/h, 50N; ISO 306
Glass Transition Temp, Tg 55.0 °C10°C/min; ISO 11357-1/-2
Flame Spread 14.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 °COptimum, Injection
 240 - 260 °CRange, Injection
Mold Temperature 80.0 °COptimum, Injection
 30.0 - 130 °CInjection
Ejection Temperature 170 °CInjection
Drying Temperature 120 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.040 %Injection
Hold Pressure >= 60.0 MPaInjection
 
Descriptive Properties
Back pressureAs low as possible
Drying RecommendedyesInjection
FMVSS ClassSE/BISO 3795 (FMVSS 302)
Part Marking Code>PBT<ISO 11469
PolymerPBT
Processing Hold Pressure Time (s/mm)4Injection
Resin IdentificationPBTISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Crastin® CE2055 BK580 Polybutylene Terephthalate (PBT)
Celanese Crastin® S600F20 NC010 PBT
BASF Ultradur® B 4040 G3 HT BK5830 15% Glass Filled PBT/PET
Celanese Crastin® S610SF BK851 Polybutylene Terephthalate (PBT)
DuPont Mobility and Materials Crastin® CE2061 BK560 PBT

PDSY5010 / 160852

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.