MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Eastman Tritan™ LX500 Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Product Description: Eastman Tritan™ LX500 is an amorphous copolyester specifically developed for use in blow molding applications for the cosmetic, fragrance, and personal care markets. Its most outstanding features are excellent toughness, hydrolytic stability, and heat and chemical resistance. In addition, this new generation copolyester offers excellent appearance and clarity.

Application/Uses:

  • Cosmetics hot-fill packaging
  • Cosmetics/personal care packaging
  • Fragrance packaging
Key Attributes:
  • Ease of processing
  • Excellent clarity
  • Fast drying times
  • Good chemical resistance
  • Good heat resistance
  • Outstanding impact resistance
  • Quick cycle times

Information provided by Eastman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³ASTM D792
Linear Mold Shrinkage 0.0060 cm/cm0.0060 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 110110ASTM D785
Tensile Strength at Break 51.0 MPa7400 psiISO 527
 52.0 MPa7540 psiASTM D638
Tensile Strength, Yield 45.0 MPa6530 psiASTM D638
 45.0 MPa6530 psiISO 527
Elongation at Break 139 %139 %ASTM D638
 142 %142 %ISO 527
Elongation at Yield 7.0 %7.0 %ASTM D638
 7.0 %7.0 %ISO 527
Tensile Modulus 1.569 GPa227.6 ksiISO 527
 1.609 GPa233.4 ksiASTM D638
Flexural Strength 60.0 MPa8700 psiISO 178
Flexural Yield Strength 64.0 MPa9280 psiASTM D790
Flexural Modulus 1.494 GPa216.7 ksiISO 178
 1.522 GPa220.7 ksiASTM D790
Izod Impact, Notched 8.42 J/cm15.8 ft-lb/inASTM D256
Izod Impact, Unnotched NBNBASTM D4812
Izod Impact, Notched (ISO)  12.0 kJ/m²
@Temperature -40.0 °C
5.71 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 78.0 kJ/m²
@Temperature 23.0 °C
37.1 ft-lb/in²
@Temperature 73.4 °F
ISO 180
Puncture Energy  62.0 J
@Temperature 23.0 °C
45.7 ft-lb
@Temperature 73.4 °F
Energy @ Max. Load; ASTM D3763
 65.0 J
@Temperature 0.000 °C
47.9 ft-lb
@Temperature 32.0 °F
Energy @ Max. Load; ASTM D3763
 67.0 J
@Temperature -40.0 °C
49.4 ft-lb
@Temperature -40.0 °F
Energy @ Max. Load; ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 101 °C214 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C185 °FASTM D648
 
Optical PropertiesMetricEnglishComments
Haze <= 1.0 %<= 1.0 %ASTM D1003
Transmission, Visible 91 %91 %ASTM D1003
 
Processing PropertiesMetricEnglishComments
Melt Temperature 235 - 255 °C455 - 491 °FEBM Processing
 260 - 280 °C500 - 536 °FISBM Processing
Mold Temperature 15.0 - 50.0 °C59.0 - 122 °FEBM Blow Mold
 35.0 - 55.0 °C95.0 - 131 °FISBM Blow Mold
 40.0 - 65.0 °C104 - 149 °FISBM Injection
Drying Temperature 88.0 °C190 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Eastman Tritan™ MX731 Medical Grade Copolyester
Avient Versaflex™ OM 2262 Thermoplastic Elastomer (TPE)
Eastman Tritan™ EX501 Copolyester
Eastman Tritan™ GX100 Copolyester
Eastman Tritan™ LX100 Copolyester

PEATM5196 / 222390

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.