MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Garlock 5500 Compressed Inorganic Fiber Gasketing, Nitrile Binder
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Inorganic fibers with a nitrile binder.
  • Inorganic fiber gasketing offers excellent thermal stability with minimal weight loss
  • Reduced creep relaxation and improved torque retention provide optimal sealability
  • Temperature resistant
  • Non-oxidizing fibers
  • IFG® 5500 has passed the Garlock Fire Test and is ABS Fire Safe Type Approved.
Media: Water, Aliphatic hydrocarbons, Oils, Gasoline, Saturated steam, Inert gases, Most refrigerants

Information provided by Garlock Rubber Technologies

Key Words: butadiene acrylonitrile
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.76 g/cc0.0637 lb/in³
Permeability 0.0500.050Gas Permeability, cc/min; DIN 3535 Part 4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 10.3 MPa1500 psiacross grain; ASTM F152
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength  9.65 kV/mm
@Temperature 121 °C,
Time 10800 sec
245 kV/in
@Temperature 250 °F,
Time 3.00 hour
0.125 in. thickness; ASTM D149
 11.2 kV/mm
@Temperature 121 °C,
Time 10800 sec
284 kV/in
@Temperature 250 °F,
Time 3.00 hour
0.0625 in. thickness; ASTM D149
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 427 °C800 °F
 288 °C
@Pressure 8.27 MPa
550 °F
@Pressure 1200 psi
Continuous
Minimum Service Temperature, Air -73.3 °C-100 °F
 
Descriptive Properties
ColorGray
Compressibility, %7-17ASTM F36
Creep Relaxation, %15ASTM F38
Sealability ASTM F37B, ml/hr0.2ASTM Fuel A
 1Nitrogen

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Nitrile Rubber (NBR, Acrylonitrile-Butadiene Rubber)
Garlock 362 Nitrile Sheet Rubber
Garlock 361 Nitrile Sheet Rubber
Garlock 5360 Nitrile Sheet Rubber
Garlock 9200 Nitrile Rubber Gasketing, Nylon Insert

PGARL842 / 157507

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.